Natural Cork Stoppers from Bark

Cork is the outer bark of the cork oak, stripped from the living tree every nine years. Cork makers stack the planks outdoors for at least six months, boil them for an hour to clean them and make them flat and springy, let them settle, then cut strips and punch stoppers out with a tube parallel to the bark's surface, so the pores, which run through the bark's thickness, cross the cork instead of running along it. A stopper is cut wider than the bottle's bore and squeezed into it: that pressure is the seal.
Miðlungs
1 day, plus 6 months seasoning

Leiðbeiningar

1

Season the planks

Stack raw cork bark planks outdoors, off the ground, for at least six months so they settle to an even moisture.

Efni fyrir þetta skref:

KorkbarkarflekiKorkbarkarfleki2 kg
2

Boil for an hour

Cut the planks to fit your largest pot, cover them with water, weigh them under with clean stones, and boil for one hour. Lift them out with tongs.

Efni fyrir þetta skref:

VatnVatn10 lítrar

Nauðsynleg verkfæri:

Stór potturStór pottur
HitaplataHitaplata
Þungir steinarÞungir steinar
Langskefta töngLangskefta töng
Hitaþolnir hanskarHitaþolnir hanskar
HandsögHandsög
3

Let them settle

Lay the boiled planks flat under a light weight in a shaded, airy place until they are dry and flat.

Nauðsynleg verkfæri:

LóðLóð
4

Cut strips

Measure the bottle's bore. Use only bark thicker than the stopper's diameter. Cut strips as wide as the stopper is long.

Nauðsynleg verkfæri:

Stafrænn skífmælir 6 tommurStafrænn skífmælir 6 tommur
DúkahnífurDúkahnífur
HandsögHandsög
5

Punch the stoppers

Fit a cork borer a few millimetres wider than the bore in the drill press. Stand the strip on edge so the borer runs between its two cut faces, parallel to the bark's surface. Push the stopper out of the tube.

Nauðsynleg verkfæri:

KorkborKorkbor
SúluborSúlubor
Stafrænn skífmælir 6 tommurStafrænn skífmælir 6 tommur
6

Smooth and fit

Sand the ends flat and chamfer the bottom edge. Test one in a bottle: it should go in with firm pressure and not leak when the bottle is laid on its side with water in it.

Nauðsynleg verkfæri:

SandpappírsörkSandpappírsörk
Glerflaska (glær)Glerflaska (glær)
7

Troubleshooting

Cork stopper troubleshooting.

Flow

Loading...

Efni

2
  • Staðgengill
  • 10 lítrar
    Staðgengill

Nauðsynleg verkfæri

13

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...