Platinum Reforming Catalyst: 0.1 % Platinum and 1.5 % Fluorine on Alumina (Haensel, UOP, US 2,479,110)
Haensel's reforming catalyst: a trace of platinum, only 0.1 %, on alumina that also carries fluorine. The fluorine is what makes it work: on the same naphtha it lifted the reformate from octane 59.8 to 78.8.
Variable: fluorine content. Tested on a Pennsylvania naphtha of octane 41.8: no fluorine 59.8; 1.5 % 78.8 (874 °F); 3 % 77.4 (824 °F); 6 % 72.4 (755 °F). Keep it at about 3 % or below.
Source: Haensel, US 2,479,110 (1949), Ex. I-II and IV. Not given: amounts of the aluminium salt and ammonia. Unknown: how the aluminium chloride hexahydrate, chloroplatinic acid and hydrogen sulfide are made. Danger: hydrofluoric acid and hydrogen sulfide are deadly poisons. Picture drawn by Youblob.
Sérfræðingur
3 days
Hættulegt efni
Þessi teikning inniheldur hættulegar aðferðir. Skráðu þig inn og virkjaðu hættulegt efni í stillingum reikningsins til að sjá skref-fyrir-skref leiðbeiningar.
Skrá innÞessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.