Potassium Bromide: Iron Bromide and Potash

Potassium bromide is the bromide of photography. Thorpe (1913): iron bromide solution run into hot potash solution until it is just neutral throws down the iron as oxide and leaves potassium bromide in solution, which is filtered, evaporated and crystallised. 100 parts of iron bromide take 56 to 60 parts of potash. The picture: potassium bromide crystals (Wikimedia Commons).
Miðlungs
2 days

Leiðbeiningar

1

Make the two solutions

Dissolve the iron bromide in water and filter it. Dissolve 56 to 60 g of potash, according to its purity, in a little water and heat it.

Efni fyrir þetta skref:

JárnbrómíðJárnbrómíð100 g
Kalíumkarbónat (pottaska)Kalíumkarbónat (pottaska)60 g

Nauðsynleg verkfæri:

VatnVatn
Grófur baðmullarsíudúkurGrófur baðmullarsíudúkur
SteypujárnspotturSteypujárnspottur
SkálavogSkálavog
2

Run the iron bromide into the potash

Pour the iron bromide solution into the hot potash until the liquid is exactly neutral or very faintly alkaline. Iron oxide falls out.

Nauðsynleg verkfæri:

SteypujárnspotturSteypujárnspottur
LakmúspappírLakmúspappír
GúmmíhanskarGúmmíhanskar
3

Boil and filter

Boil for some time so the iron oxide settles dense, then filter it off.

Nauðsynleg verkfæri:

SteypujárnspotturSteypujárnspottur
Grófur baðmullarsíudúkurGrófur baðmullarsíudúkur
4

Dry, then dissolve again

Evaporate to dryness. Dissolve the residue again in water: potassium sulphate and other dirt stay behind. Filter.

Nauðsynleg verkfæri:

SteypujárnspotturSteypujárnspottur
VatnVatn
Grófur baðmullarsíudúkurGrófur baðmullarsíudúkur
5

Crystallise

Boil down to specific gravity 1.53, then evaporate further at a gentle heat in a stoneware or enamelled dish, for hard crystals.

Nauðsynleg verkfæri:

SteypujárnspotturSteypujárnspottur
FlotvogFlotvog
UppgufunarskálUppgufunarskál
6

Dry at 40 to 50 °C

Dry the crystals at 40 to 50 °C, not above, or they crackle and burst.

Nauðsynleg verkfæri:

UppgufunarskálUppgufunarskál
HitamælirHitamælir

Efni

2

Nauðsynleg verkfæri

9

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...