PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)
Charlie

Búin til af

Charlie

28. október 2026DE
6
0
0
0
0

PTFE Fine Powder: a Dispersion Stirred Until It Curdles (Lontz 1952)

A PTFE dispersion is stable on the shelf, but stirred hard enough it curdles. Fifty seconds at 1000 rpm in a baffled beaker and the polymer floats up as a dry-looking, unwettable crumb. Washed and dried, it is a free-flowing powder for rolling into tape, or for cold lubricated extrusion. Source: J. F. Lontz (du Pont), US 2,593,583 (1952), Example 1. Lontz started from a dispersion made with disuccinic acid peroxide; ours is Berry's persulfate dispersion, diluted to his 17 %. Picture drawn by Youblob.
Miðlungs
1 day

Leiðbeiningar

1

Dilute the dispersion to 17 %

Ours: stir the 34 % dispersion with an equal weight of distilled water to get 17 % solids, the strength Lontz used.

Efni fyrir þetta skref:

PTFE-vatnsdreifaPTFE-vatnsdreifa1 part
Eimað vatnEimað vatn1 part

Nauðsynleg verkfæri:

SkálavogSkálavog
Glerkrukka með lokiGlerkrukka með loki
2

Set up the baffled beaker

A 1-gallon stainless beaker, 6.5 in across and 7.5 in deep, with four baffles about ⅜ × 1 in hanging from the cover to within 3 in of the bottom. Stirrer: open turbine, 4 blades 1½ in high, 5 in across, reaching to within 1 in of the bottom.

Nauðsynleg verkfæri:

Hræritankur með brotplötumHræritankur með brotplötum
HrærariHrærari
3

Stir hard at 176 °F for 50 seconds

Put in half a gallon of the 17 % dispersion and heat it to 176 °F (80 °C). Run the stirrer at 1000 rpm for 50 seconds (Lontz measured 0.72 hp per gallon). The polymer coagulates and floats, unwetted, on top.

Nauðsynleg verkfæri:

Hræritankur með brotplötumHræritankur með brotplötum
HrærariHrærari
HitaplataHitaplata
HitamælirHitamælir
4

Wash hot, then cold

Pour off the water. Wash the polymer with hot water at 176 °F, then with cold water at 60 °F (16 °C), and drain.

Nauðsynleg verkfæri:

Hræritankur með brotplötumHræritankur með brotplötum
HitamælirHitamælir
5

Dry at 230 °F for 16 hours

Spread the wet polymer on a 100-mesh screen and dry it in an oven at 230 °F (110 °C) for 16 hours. It comes out a free-flowing granular powder that passes 6–8 mesh.

Nauðsynleg verkfæri:

Sigti með fínu vírnetiSigti með fínu vírneti
ÞurrkofnÞurrkofn
Glerkrukka með lokiGlerkrukka með loki

Efni

2

Nauðsynleg verkfæri

8

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.