Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)
Forge

Búin til af

Forge

4. nóvember 2026NO
13
0
0
0
0

Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)

The file for sharpening saw teeth as Sheffield made it by hand: a three-square (triangular) bar of cast steel, not tapering, forged in a V-shaped boss, its teeth cut one by one with a chisel and hammer, then hardened under a coat of animal carbon and salt and quenched in cold spring water. Ure says saw files in particular should be hardened with the carbon mixture, so they will cut iron and steel. Not given: sizes and teeth per inch. Source: A. Ure, Dictionary of Arts, Manufactures, and Mines (1839), File. Picture: our drawing.
Lengra kominn
Unknown

Leiðbeiningar

1

Forge the blank

Draw cast steel out square at the forge, then lay it with one angle down in a boss whose recess has two sides meeting at an angle, so the hammer forms one side and the boss the other two. Keep it the same size along its length (saw files are not tapered).

Efni fyrir þetta skref:

DeiglustálDeiglustál1 cast steel bar
Óþekkt málÓþekkt mál1 stykki

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
SmiðjutöngSmiðjutöng
Neðri mótsteðji (neðra mót)Neðri mótsteðji (neðra mót)
HamarHamar
SleggjaSleggja
2

Cut the teeth

On an anvil with a flat, even face, hold the file down with a leather strap over each end, the workman's feet in the straps like stirrups. Cut the teeth with a chisel a little broader than the file, sharpened to about 20 degrees, struck with a hammer of 1 to 6 lb. For single cut, run a fine file lightly over the teeth to take off the roughness; for double cut, cut a second set nearly at right angles to the first.

Nauðsynleg verkfæri:

StálsteðjiStálsteðji
LeðurólLeðuról
KaldmeitillKaldmeitill
HamarHamar
MálmþjölMálmþjöl
3

Cut the other sides

To cut the next side, lay the file in a piece of lead-tin alloy with an angular groove, so the teeth already cut are not spoiled on the anvil.

Nauðsynleg verkfæri:

Tin-blý lóðmálmurTin-blý lóðmálmur
StálsteðjiStálsteðji
KaldmeitillKaldmeitill
HamarHamar
4

Coat for hardening

Distil shoemakers' and curriers' leather refuse in an iron still and powder the bright coal left. Grind about equal parts by bulk of this carbon and salt to the consistence of cream with water and cover the file with it.

Nauðsynleg verkfæri:

JárnkolbaJárnkolba
SaltSalt
VatnVatn
5

Harden

Hold the file by the tang in a fire of very small cokes, drawing it out often, until it is an even cherry red from tang to point. Plunge it straight down, quickly, into clear spring water as cold as possible.

Nauðsynleg verkfæri:

SmiðjueldstæðiSmiðjueldstæði
MálmvinnslukoxMálmvinnslukox
SmiðjutöngSmiðjutöng
VatnVatn
6

Clean and oil

Brush the file with water and powdered cokes until clean and metallic, wash it in two or three waters to take off all the salt, dip it in lime-water, dry it quickly before the fire and oil it while warm with olive oil containing a little oil of turpentine.

Nauðsynleg verkfæri:

MálmvinnslukoxMálmvinnslukox
VatnVatn
KalkvatnKalkvatn
ÓlífuolíaÓlífuolía
TerpentínaTerpentína

Efni

2
  • 1 cast steel bar
    Staðgengill
  • Staðgengill

Nauðsynleg verkfæri

17

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...