Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)
Charlie

Búin til af

Charlie

31. október 2026DE
1
0
0
0
0

Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)

Paper soaked in phenol resin is dried, then cured only part of the way, so the resin is stiff but not yet hard. Lucas did this before the final hot press so the press would not squeeze the resin out of the fibres. Result: a dry, partly cured phenolic sheet that a later coat of phenolic resin can still bond into. Source: Lucas, US 1,470,990 (Western Electric, 1923). Stopping before his final hot press is ours. Not given: the solvent in his resin, paper grade, mercerising strengths. Picture drawn by Youblob.
Miðlungs
1 hour

Leiðbeiningar

1

Dip the paper in phenol resin

Run the paper through a bath of phenol resin of specific gravity about 0.970: about 2 minutes for plain paper, 1 minute or less if mercerised first. Ours: Liquid Bakelite as the resin; Lucas does not say how it was thinned.

Efni fyrir þetta skref:

PappírPappír1 as required
Fljótandi bakelít (þéttiafurð fenóls og formaldehýðs)Fljótandi bakelít (þéttiafurð fenóls og formaldehýðs)1 as required

Nauðsynleg verkfæri:

Gegndreypingarlína fyrir prepregGegndreypingarlína fyrir prepreg
FlotvogFlotvog
2

Optional: mercerise the paper first

For faster, fuller soaking, first pass the paper through caustic soda, squeeze, wash in water, neutralise in an acid, wash again and dry. Strengths and the acid: not given.

Nauðsynleg verkfæri:

Vítissódi (natríumhýdroxíð)Vítissódi (natríumhýdroxíð)
Gegndreypingarlína fyrir prepregGegndreypingarlína fyrir prepreg
3

Dry at about 90 °C

Dry the soaked paper in an oven at about 90 °C, just long enough to dry it.

Nauðsynleg verkfæri:

ÞurrkofnÞurrkofn
4

Part-cure at 120-130 °C

Pass the dry paper through a curing oven at 120-130 °C for about 10 minutes (Lucas's description; his claim 4 says 125 °C for about 10 seconds). The resin sets as stiff as the fibres, but does not harden through.

Nauðsynleg verkfæri:

HerðingarofnHerðingarofn
5

Dip again for 10-15 seconds and dry

Dip the part-cured paper in phenol resin again for 10-15 seconds, then dry at about 90 °C until it can be wound on a reel. Stop here: the sheet is semi-cured. Lucas's next step, stacking and hot pressing, cures it fully.

Efni fyrir þetta skref:

Fljótandi bakelít (þéttiafurð fenóls og formaldehýðs)Fljótandi bakelít (þéttiafurð fenóls og formaldehýðs)1 as required

Nauðsynleg verkfæri:

Gegndreypingarlína fyrir prepregGegndreypingarlína fyrir prepreg
ÞurrkofnÞurrkofn

Efni

2

Nauðsynleg verkfæri

5

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...