Neodymium Magnets, Sample 11: 62Fe-23B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 11, 62 % iron, 23 % boron and 15 % neodymium by atoms: 10.9 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Sérfræðingur
2 days
Leiðbeiningar
1
1
Weigh sample 11: 62 Fe, 23 B, 15 Nd
Weigh sample 11: 62 Fe, 23 B, 15 Nd
Sample 11 is 62 % iron, 23 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 426.6 g iron, 218.4 g ferroboron, 368.3 g neodymium. Unknown: how these three are made.
Efni fyrir þetta skref:
Rafgreint járn426.6 g
Járnbór218.4 g
Neódýmmálmur368.3 gNauðsynleg verkfæri:
Skálavog2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Nauðsynleg verkfæri:
Spanofn
Deigla úr eldföstum leir
Argon
Þrýstigaskútur
Vatnskælt koparmót
Hitaþolnir hanskar3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Nauðsynleg verkfæri:
Stappmylla
Sigtasett (stigskipt möskvastærð)
Járnkúlukvörn
Öryggisgleraugu4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Nauðsynleg verkfæri:
Segulsviðspressa5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 11 measured 6.8 kG remanence, 11.3 kOe coercivity and 10.9 MGOe.
Nauðsynleg verkfæri:
Pípuofn
Argon
Þrýstigaskútur
Hitaþolnir hanskar6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
Nauðsynleg verkfæri:
Óþekkt segulmögnunaraðferðEfni
3- 426.6 gStaðgengill
- 218.4 gStaðgengill
- 368.3 gStaðgengill
Nauðsynleg verkfæri
14- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
Þessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.