Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)
Forge

Búin til af

Forge

1. nóvember 2026NO
5
0
0
0
0

Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)

The renowned bar iron of Dannemora was refined in the old Walloon way: long white pigs melt drop by drop before a cold blast in a small, very hot charcoal hearth, the finer works the metal with an iron staff until it comes to nature, and the lump is drawn out under water-driven hammers. Result: bars 12 ft long of about 60 lb; 6 tons a week from one hearth, 80 % of the weight of the pig. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 599-601, after Tunner and A. Grill. Picture drawn by Youblob.
Sérfræðingur
about 30 minutes per lump; 8-hour shifts

Leiðbeiningar

1

Build the finery hearth

Make the hearth of cast-iron plates: a 2-inch bottom plate on about 3 inches of pounded slag, over a cast-iron box with channels to drain water. From the tuyere it is 10-11½ inches to the back-plate, 22-24 inches to the work-plate and 22-24 inches to the opposite side. Depth: 7-8 inches under the tuyere, 14-15 under the back-plate, 15-18 opposite the tuyere. No tapping hole: the slag is never let out.

Nauðsynleg verkfæri:

HreinsiaflHreinsiafl
2

Set the tuyere and blast

The tuyere nozzle is semicircular, flat side down, 20-25 lines broad and 16-17 lines high, and projects 3½ inches; the blast-pipe nozzle sits 4 inches back inside it. Use cold blast. The blowing machine is not described.

Nauðsynleg verkfæri:

HreinsiaflHreinsiafl
SmiðjubelgurSmiðjubelgur
3

Lay in the pigs

Use white or strongly mottled pig in long pigs about 9 inches broad, 15-18 feet long, 3-4 inches thick at one end and 1-2 at the other. Lay them across the back-plate, one end sloping down over the tuyere, usually two one above the other, and push them forward as the ends melt.

Efni fyrir þetta skref:

Hvítt viðarkolasteypujárnHvítt viðarkolasteypujárn1 long pigs

Nauðsynleg verkfæri:

HreinsiaflHreinsiafl
4

Light and make the slag bath

Fill the front of the hearth with moistened small charcoal and the rest with charcoal, light it and turn on the blast. To make enough slag bath, melt down some large finery scraps or, failing these, several shovelfuls of hammer scale.

Nauðsynleg verkfæri:

Viðarkol - fínmöluðViðarkol - fínmöluð
VatnVatn
ViðarkolViðarkol
JárnhamarshreisturJárnhamarshreistur
SkóflaSkófla
5

Reheat the last bloom

At the start of each heat, hold the bloom from the last lump with tongs, as steeply as you can, in the front of the hearth to reheat it for drawing out.

Nauðsynleg verkfæri:

SmiðjutöngSmiðjutöng
6

Work the metal with the staff

As soon as the first pig iron melts, work it with an iron staff: bring the metal on the tuyere side up from the bottom towards the middle into the blast, once to the left and once to the right of the reheating bloom. About 70 lb melts in 20 minutes; thin pieces of malleable iron then cling to the staff.

Nauðsynleg verkfæri:

JárnteinnJárnteinn
7

Form the lump

Stop the flow of fresh molten pig, break up all the metal above the tuyere, melt it down and gather it into a lump about 12 by 15 inches. One lump takes 28 minutes on average (25-30).

Nauðsynleg verkfæri:

JárnteinnJárnteinn
SmiðjutöngSmiðjutöng
8

Draw out the bar

Heat each lump 6-8 times in a separate fire and draw it out under water-driven hammers into a bar 12 feet long of about 60 lb. One finery, one drawing-out forge and one hammer make 6 tons of bars a week; the bars weigh 80 % of the pig, and take 3 tons of charcoal per ton.

Nauðsynleg verkfæri:

AflinnAflinn
KambhamarKambhamar
VatnshjólVatnshjól
SmiðjutöngSmiðjutöng

Efni

1

Nauðsynleg verkfæri

12

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...