Arthur F. Payne · Public domain (1914)
Teaspoon Forged from a Silver Bar (Payne 1914)
A 6-inch silver teaspoon forged out of a small bar of silver, the way a blacksmith forges iron. Arthur Payne called it the hardest of his five spoon methods, but the cheapest, because almost no silver is wasted.
Source: A. F. Payne, Art Metalwork with Inexpensive Equipment (1914), pp. 184–186; annealing from his chapter XI. Cutting the bar from sheet is ours. Picture: Payne's Fig. 158, teaspoons forged this way.
Lengra kominn
1 day
Leiðbeiningar
1
1
Cut the silver bar
Cut the silver bar
For a teaspoon 6 in long you need a piece of sterling silver 4 in long, ½ in wide and ⅛ in thick. Mark it out and saw it from sheet of that thickness (cutting from sheet is ours).
Efni fyrir þetta skref:
Plata úr sterlingsilfri1 piece 4 × ½ × ⅛ inNauðsynleg verkfæri:
Rissnál
Gullsmíðasög2
2
Forge out the bowl
Forge out the bowl
Heat the bar until it is almost red-hot, hold it in tongs and forge the bowl out on the anvil. Silver forges more easily when it is nearly red, but never hammer it while it is red-hot: it will crack.
Nauðsynleg verkfæri:
Bunsenbrennari
Töng
Steðji
Hamar3
3
Work bowl, then shank and handle
Work bowl, then shank and handle
Hammer the bowl until it is hard, then the shank and handle, so the whole spoon is hard before you anneal it again. That saves time.
Nauðsynleg verkfæri:
Steðji
Hamar4
4
Anneal and repeat
Anneal and repeat
To soften it, heat it to a dull red and plunge it into water, or let it cool. Then go on forging until the spoon is roughly to shape.
Efni fyrir þetta skref:
Vatn1 as requiredNauðsynleg verkfæri:
Bunsenbrennari
Töng
Glerílát5
5
Trim with shears and file
Trim with shears and file
Trim the outline with the shears and file the edges smooth.
Nauðsynleg verkfæri:
Sterk málmklippa
Þjalir (handþjöl)6
6
Polish out the file marks
Polish out the file marks
Rub out all the scratches and file marks with emery cloth.
Nauðsynleg verkfæri:
Smergildúkur7
7
Anneal to even the fire scale
Anneal to even the fire scale
Anneal the spoon thoroughly once more. Heated silver grows a thin white skin, the fire scale, and this brings it back over the spots where filing and polishing took it off, so the colour is even.
Efni fyrir þetta skref:
Vatn1 as requiredNauðsynleg verkfæri:
Bunsenbrennari
Töng
Glerílát8
8
Planish with smooth hammers
Planish with smooth hammers
Planish the spoon on smooth tools with smooth, bright hammers. This makes it stiff again after the annealing.
Nauðsynleg verkfæri:
Sléttihamar
Steðji
Hæll9
9
Final polish with rouge
Final polish with rouge
Polish it lightly with a soft cotton flannel and a little red rouge.
Nauðsynleg verkfæri:
Fægiklútur fyrir skartgripi
GullsmiðarauttNauðsynleg verkfæri
14- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
- Staðgengill
Þessi teikning býr til
Tengd Blueprint
Þessi blueprint deila þekkingu — tækni, efni eða meginreglur
CC0 opinbert ríki
Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.
Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.