Violet Iron Oxide: Precipitated Hematite Calcined at 1000-1100 °C (Nurdini et al. 2022)

Iron hydroxide is thrown down from hot ferric nitrate solution with ammonia, washed, dried and calcined. All of it ends as pure hematite, but the colour moves from bright red through dark red to purple as the calcining heat rises from 1000 °C, because the grains grow larger and more crystalline. Result: pure violet to purple ferric oxide (hematite) after 4 hours at 1000-1100 °C. Source: Nurdini et al., Heliyon 8 (2022) e10377, sections 2.2 and 4. Not given: batch size, how much ammonia, end pH, yield. Picture drawn by Youblob.
Miðlungs
2 days

Leiðbeiningar

1

Heat the ferric nitrate solution

Make a 0.05 M solution of ferric nitrate in distilled water and heat it to 80 °C.

Efni fyrir þetta skref:

Járn(III)nítratJárn(III)nítrat1 as required

Nauðsynleg verkfæri:

Eimað vatnEimað vatn
GlerbikarGlerbikar
HitaplataHitaplata
HitamælirHitamælir
2

Throw down the hydroxide with ammonia

Keeping it at 80 °C, add ammonia solution drop by drop while stirring well. Stir for 3 hours, then let it cool to room temperature: a red-brown precipitate forms. Not given: how much ammonia.

Nauðsynleg verkfæri:

Ammoníaklausn 25-28 %Ammoníaklausn 25-28 %
DropatrektDropatrekt
HitaplataHitaplata
HitamælirHitamælir
3

Spin down, wash and dry

Collect the precipitate in a centrifuge at 4000 rpm for 15 minutes, wash it with distilled water, and dry it at 110 °C for 24 hours.

Nauðsynleg verkfæri:

BorðskilvindaBorðskilvinda
Eimað vatnEimað vatn
ÞurrkofnÞurrkofn
4

Calcine at 1000-1100 °C

Calcine for 4 hours in air at 1000-1100 °C. Below 1000 °C it stays bright or dark red; from 1000 °C it turns purple. Grind the cooled oxide to a fine powder (they used an agate mortar).

Nauðsynleg verkfæri:

MúffluofnMúffluofn
Mortél og mortélstauturMortél og mortélstautur

Efni

1

Nauðsynleg verkfæri

10

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.

Studdu smiðinn með því að kaupa vörur í gegnum teikningu hans þar sem hann fær þóknun smiða sem seljendur ákvarða, eða búðu til nýja endurskoðun á þessari teikningu og tengdu hana sem tengingu í þinni eigin teikningu til að deila tekjum.

Umræða

(0)

Skrá inn til að taka þátt í umræðunni

Hleður athugasemdum...