Metal Oxide Varistor: Zinc Oxide with 5 % Bismuth Oxide, 1100 °C, 1.0 mm (Masuyama 1972)

A non-linear resistor: the current through it rises far faster than the voltage across it. Masuyama, Matsuoka and Nishi made one from zinc oxide with a little bismuth oxide: pressed into a disc, sintered, lapped, and given metal electrodes. With 5 mole % bismuth oxide, sintered at 1100 °C and lapped to 1.0 mm, the disc measured a C-value of 65 at 1 mA and a nonlinearity exponent n of 3.3. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 1. Unknown: how the aluminium is sprayed on and what the silver paint is. The patent calls both well known, so they are linked to unknown heads. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Lengra kominn
1 day

Leiðbeiningar

1

Weigh 95 : 5 and wet-mill 5 hours

Mix zinc oxide and bismuth oxide 95 : 5 by moles. Ours, for 10 g: 7.684 g zinc oxide, 2.316 g bismuth oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.

Efni fyrir þetta skref:

SinkoxíðduftSinkoxíðduft7.684 g
BismútoxíðBismútoxíð2.316 g

Nauðsynleg verkfæri:

SkálavogSkálavog
JárnkúlukvörnJárnkúlukvörn
ÞurrkofnÞurrkofn
2

Press discs 13 mm by 2.5 mm

Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm².

Nauðsynleg verkfæri:

VökvapressaVökvapressa
Pressumót fyrir skífurPressumót fyrir skífur
SkífmælirSkífmælir
3

Sinter 1 hour at 1100 °C and furnace-cool

Sinter the discs in air for 1 hour at 1100 °C, then let them cool in the furnace to room temperature (about 15-30 °C).

Nauðsynleg verkfæri:

MúffluofnMúffluofn
4

Lap both faces to 1.0 mm

Lap both faces with 600-mesh silicon carbide until the disc is 1.0 mm thick.

Nauðsynleg verkfæri:

KísilkarbíðkornKísilkarbíðkorn
SkífmælirSkífmælir
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.

Efni fyrir þetta skref:

ÁlhleifurÁlhleifur1 as required
Leiðandi silfurmálningLeiðandi silfurmálning1 as required
KoparvírKoparvír2 stykki

Nauðsynleg verkfæri:

Óþekkt málmúðunaraðferðÓþekkt málmúðunaraðferð
SkífmælirSkífmælir

Efni

5

Nauðsynleg verkfæri

9

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.