Metal Oxide Varistor: Pure Zinc Oxide at 1350 °C, Bismuth Oxide Paste Fired at 600 °C (Masuyama 1972, Ex. 4)
Ed

Búin til af

Ed

28. október 2026FI
3
0
0
0
0

Metal Oxide Varistor: Pure Zinc Oxide at 1350 °C, Bismuth Oxide Paste Fired at 600 °C (Masuyama 1972, Ex. 4)

A varistor made the other way round: a disc of pure zinc oxide, sintered, with bismuth oxide fired into its faces from a paste instead of mixed in. Sintered at 1350 °C and fired with the paste at 600 °C, the disc measured a C-value of 13 at 1 mA and a nonlinearity exponent n of 4.2. Masuyama found that firing on the bismuth oxide paste raises n a great deal over mixing it in. Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 4. Unknown: how the aluminium is sprayed on, what the silver paint is, and how strong the epoxy solution of the paste is. The 10 g batch is our arithmetic. Picture: the patent's drawing.
Lengra kominn
2 days

Leiðbeiningar

1

Press pure zinc oxide at 340 kg/cm²

Press zinc oxide powder at 340 kg/cm². Example 4 gives no disc size; ours: discs 13 mm across and 2.5 mm thick in the mould of Example 1.

Efni fyrir þetta skref:

SinkoxíðduftSinkoxíðduft1 as required

Nauðsynleg verkfæri:

SkálavogSkálavog
VökvapressaVökvapressa
Pressumót fyrir skífurPressumót fyrir skífur
SkífmælirSkífmælir
2

Sinter 1 hour at 1350 °C and cool

Heat the pressed disc for 1 hour at 1350 °C, then let it cool to room temperature.

Nauðsynleg verkfæri:

MúffluofnMúffluofn
3

Lap both faces

Lap both faces with silicon carbide abrasive. Example 4 gives no thickness.

Nauðsynleg verkfæri:

KísilkarbíðkornKísilkarbíðkorn
SkífmælirSkífmælir
4

Coat with bismuth oxide paste and fire at 600 °C

Coat both lapped faces with a paste of 50 % by weight bismuth oxide in a solution of epoxy resin in butyl alcohol, and fire it in air at 600 °C for 30 minutes. The bismuth oxide diffuses into the zinc oxide. Not given: how much paste, or the strength of the epoxy solution.

Efni fyrir þetta skref:

BismútoxíðBismútoxíð1 as required

Nauðsynleg verkfæri:

EpoxýkvoðaEpoxýkvoða
n-Bútanóln-Bútanól
MúffluofnMúffluofn
5

Spray aluminium electrodes and attach leads

Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint, as in Example 1. Unknown: the spraying method and the paint.

Efni fyrir þetta skref:

ÁlhleifurÁlhleifur1 as required
Leiðandi silfurmálningLeiðandi silfurmálning1 as required
KoparvírKoparvír2 stykki

Nauðsynleg verkfæri:

Óþekkt málmúðunaraðferðÓþekkt málmúðunaraðferð
SkífmælirSkífmælir

Efni

5

Nauðsynleg verkfæri

9

Tengd Blueprint

Þessi blueprint deila þekkingu — tækni, efni eða meginreglur

CC0 opinbert ríki

Þessi teikning er gefin út undir CC0. Þér er frjálst að afrita, breyta, dreifa og nota þetta verk í hvaða tilgangi sem er, án þess að biðja um leyfi.