Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass
A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding.
The picture: our diagram.
Intermedio
3 days
Istruzioni
1
1
Level the bottom plate
Level the bottom plate
Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.
Strumenti necessari:
Lastra di vetro
Telaio di legno
Gesso da presa
Livella a bolla da 1,5 m2
2
Pour the first 1/2 inch
Pour the first 1/2 inch
Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.
Materiali per questo passaggio:
Sciroppo di metacrilato di metile3 lStrumenti necessari:
Guanti di gomma
Termometro da laboratorio3
3
Pour the next layer and cover
Pour the next layer and cover
Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.
Strumenti necessari:
Lastra di vetro4
4
Heat at 80 °C
Heat at 80 °C
Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.
Strumenti necessari:
Essiccatoio
Termometro da laboratorio
Guanti resistenti al calore5
5
Spring off the glass
Spring off the glass
Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.
Strumenti necessari:
Taglierino di precisione
Guanti di gommaMateriali
1- Segnaposto
Strumenti richiesti
9- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.