Acrylic Mirror Sheet: Silver Sprayed on Acrylic Treated with Tannin in Water and Methanol
Philips' Ponjee and Verwijlen (US 4,639,382, 1987) made silver hold on acrylic by first dipping it in tannin dissolved in water mixed with an organic solvent; tannin in plain water gave no bond. This is their methanol solution: 45–70 % water, 30–55 % methanol by volume, 2.7–4.3 g tannin per litre, which gave full bonding in their cross-cut test. The sheet is then sensitised with weak stannous chloride and silvered by spraying the silver solution and the reducer together.
The picture: our diagram.
Intermedio
2 hours
Istruzioni
1
1
Dip in tannin solution for one minute
Dip in tannin solution for one minute
Make a solution of 2.7–4.3 g of tannic acid per litre in 45–70 % water and 30–55 % methanol by volume. Dip the acrylic sheet in it for one minute.
Materiali per questo passaggio:
Lastra di acrilico1 pezzoStrumenti necessari:
Acido tannico
Metanolo
Acqua distillata
Vassoi di vetro
Cilindro graduato
Bilancia a bracci
Cappa aspirante (canalizzata)
Guanti di gomma2
2
Rinse with water
Rinse with water
Rinse the sheet with water.
Strumenti necessari:
Acqua distillata
Spruzzetta da laboratorio3
3
Spray with stannous chloride for 12 seconds
Spray with stannous chloride for 12 seconds
Spray the face to be silvered with a solution of 0.1 g stannous chloride and 0.1 ml concentrated hydrochloric acid per litre of water, for 12 seconds. Rinse off the excess with water.
Strumenti necessari:
Cloruro stannoso
Acido cloridrico
Acqua distillata
Spruzzino ad acqua
Spruzzetta da laboratorio
Occhiali antispruzzo chimico
Guanti di gomma4
4
Spray silver and reducer together
Spray silver and reducer together
Atomise two solutions onto the face at the same time: silver nitrate with ammonia in water, and formalin in water. The patent gives no strengths: as required. Ours: a twin-nozzle spray gun.
Materiali per questo passaggio:
Nitrato d'argento1 as requiredStrumenti necessari:
Soluzione di ammoniaca al 25-28 %
Soluzione di formaldeide (formalina al 37 %)
Acqua distillata
Pistola a spruzzo a doppio ugello
Cappa aspirante (canalizzata)
Occhiali antispruzzo chimico
Guanti di gommaMateriali
2- 1 pezzoSegnaposto
- 1 as requiredSegnaposto
Strumenti richiesti
16- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.