Activated Alumina: Aluminium Trihydrate Heated at 350 °C While Hot Air Carries the Steam Away (Derr, Alcoa, US 2,015,593)
Heating aluminium trihydrate drives out its water and leaves a porous alumina that soaks up moisture. Alcoa's Derr found it works much better when the steam is carried away at once, by a stream of hot air or by a vacuum, instead of lingering in the bed.
Result: activated alumina that takes up 14 % of its weight in water from air (8 % made the old way), up to 16 % if washed first in 3 % sulphuric acid.
Source: Derr, US 2,015,593 (Alcoa, 1935). Not given: times, bed depth, air rate, amounts. Picture drawn by Youblob.
Intermedio
1 day
Istruzioni
1
1
Wash the trihydrate in 3 % sulphuric acid
Wash the trihydrate in 3 % sulphuric acid
Before heating, wash the aluminium trihydrate in water containing about 3 % by weight of sulphuric acid. Derr calls this very desirable but not essential: it raises the capacity by about 1-2 %. Ours: stir in a beaker.
Materiali per questo passaggio:
Idrossido di alluminio1 as requiredStrumenti necessari:
Acido solforico diluito
Acqua
Becher in borosilicato
Bacchetta di vetro2
2
Lay it in beds in a chamber
Lay it in beds in a chamber
Put the material in beds or layers in a chamber that gas can be drawn through. Ours: a tube furnace.
Strumenti necessari:
Forno a tubo3
3
Draw air at 350 °C through the bed
Draw air at 350 °C through the bed
Draw air (or combustion gas) heated to about 350 °C through the bed and out of the chamber in a continuous flow, so the steam leaves at once. Temperature: 250-800 °C works, 350-400 °C is best; above 800 °C the alumina changes and loses capacity.
Strumenti necessari:
Soffiatore d'aria
Pirometro4
4
Or heat it under a partial vacuum
Or heat it under a partial vacuum
Instead of hot air, close the chamber, keep a partial vacuum in it and heat above 250 °C and below 800 °C; 300-400 °C on a large scale. The steam passes quickly out of the chamber.
Strumenti necessari:
Pompa per vuoto
Pirometro5
5
Keep it dry
Keep it dry
The product takes up about 14 % of its weight of water from air, 16 % if acid-washed. Ours: store it in an airtight container until use.
Strumenti necessari:
Contenitori ermeticiMateriali
1- 1 as requiredSegnaposto
Strumenti richiesti
9- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- 1 vendor sell this, none ship to you yetSegnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.