Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)
Ordinary soaps stop tetrafluoroethylene from growing into long chains. A fluorine soap does not: with 2 % of ammonium dodecafluoroheptanoate in the water, the gas polymerises into tiny PTFE ribbons that stay suspended. The result is a milky dispersion, a third of it polymer, the raw material for PTFE fine powder.
Source: K. L. Berry (du Pont), US 2,559,752 (1951), Example III. Making the ammonium salt from our acid, and the apparatus, are ours. Picture drawn by Youblob.
Avanzato
1 day
Istruzioni
1
1
Make the ammonium salt
Make the ammonium salt
Ours: neutralise about 1.9 parts of dodecafluoroheptanoic acid with ammonia solution until just neutral to litmus, giving 2 parts of ammonium dodecafluoroheptanoate. Make it up with distilled water to 93 parts of water in all. Parts are by weight.
Materiali per questo passaggio:
Acido dodecafluoroeptanoico1.9 parts
Soluzione di ammoniaca al 25-28 %1 as required to neutralise
Acqua distillata93 partsStrumenti necessari:
Cartina al tornasole
Recipiente di vetro
Bilancia a bracci2
2
Load the pressure vessel
Load the pressure vessel
Put the solution in a pressure vessel with 0.05 part of potassium persulfate and 5 parts of paraffin wax melting at 56–58 °C. The wax protects the colloid while it is stirred.
Strumenti necessari:
Iniziatore a persolfato
Paraffina
Reattore a pressione
Bilancia a bracci3
3
Heat and remove the air
Heat and remove the air
Bring it to 80–85 °C, then evacuate the vessel and hold it under reduced pressure for several minutes to drive out air and dissolved oxygen.
Strumenti necessari:
Reattore a pressione
Pompa per vuoto
Termometro4
4
Feed tetrafluoroethylene for 3.6 hours
Feed tetrafluoroethylene for 3.6 hours
Let in tetrafluoroethylene to 60 lb/sq in gauge. Agitate at 80–85 °C for 3.6 hours; each time the pressure falls to 55 lb/sq in, bring it back to 60.
Materiali per questo passaggio:
Tetrafluoroetilene1 as required to hold 55–60 psiStrumenti necessari:
Reattore a pressione
Bombola di gas in pressione
Manometro
Termometro5
5
Cool and lift off the wax
Cool and lift off the wax
Cool it. The paraffin sets on top and lifts off. Below it is a colloidal PTFE dispersion with 34 % solids.
Strumenti necessari:
Reattore a pressione
Barattoli di vetro con coperchioMateriali
4- 1.9 partsSegnaposto
- 1 as required to neutraliseSegnaposto
- 93 partsSegnaposto
- 1 as required to hold 55–60 psiSegnaposto
Strumenti richiesti
11- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- 1 vendor sell this, none ship to you yetSegnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi

Pericoloso
Dodecafluoroheptanoic Acid: the Fluoro Alcohol Oxidised with Permanganate (Berry 1951)
di Charlie
Industriale
7
0
0
0
0
0

Pericoloso
Tetrafluoroethylene: Chlorodifluoromethane Pyrolysed in a Silver Tube at 700 °C
di Charlie
Industriale
12
0
0
0
0
0

PTFE Resin Powder: Tetrafluoroethylene Polymerised under Pressure, Plunkett 1941
di Charlie
Industriale
12
0
0
0
0
0
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.