Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)
Charlie

Creato da

Charlie

28. ottobre 2026DE
6
0
0
0
0

Barium Ferrite Disc Magnet: Fired in Carbon Dioxide, Pressed at 12 t/cm² (Went, Philips 1956, Ex. 33)

A barium ferrite made with more iron oxide, 0.4 mol barium carbonate to 3.6 mol, fired an hour at 1300 °C in carbon dioxide. Little oxygen gives the hexagonal crystal BaFe18O27, with some iron in the lower state. It is milled again, bound with nitrocellulose or polyvinyl alcohol, and pressed hard at 12 tonnes per cm². Went's rod held 1,260 gauss with a coercive force of 700 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 33. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzato
2 days

Istruzioni

1

Weigh barium carbonate and iron oxide

Weigh 79.4 g barium carbonate (0.4 mol) and 580.9 g ferric oxide (3.6 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

Materiali per questo passaggio:

Carbonato di bario (witherite)Carbonato di bario (witherite)79.4 g
Ossido ferricoOssido ferrico580.9 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Guanti di gommaGuanti di gomma
Respiratore P100Respiratore P100
2

Mill 15.5 hours, press a pastille, fire in CO2

Grind with alcohol in a ball mill for 15.5 hours, dry, and press into a pastille. Heat it at 1300 °C in carbon dioxide for 1 hour (ours: a tube furnace fed from a CO2 cylinder).

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Etanolo per laboratorio, 95 %Etanolo per laboratorio, 95 %
EssiccatoioEssiccatoio
Pressa idraulicaPressa idraulica
Stampo per pressatura di dischiStampo per pressatura di dischi
Forno a tuboForno a tubo
Anidride carbonica gassosaAnidride carbonica gassosa
Bombola di gas in pressioneBombola di gas in pressione
Guanti resistenti al caloreGuanti resistenti al calore
3

Pulverise, mill 14 hours, bind

Crush the cooled pastille and grind it with alcohol for 14 hours. Press the powder into a pastille again with a ceramic binder (ours: polyvinyl alcohol, one of the two named), then crush it to grains.

Materiali per questo passaggio:

Alcol polivinilico in polvereAlcol polivinilico in polvere1 as required

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Etanolo per laboratorio, 95 %Etanolo per laboratorio, 95 %
Pressa idraulicaPressa idraulica
Stampo per pressatura di dischiStampo per pressatura di dischi
4

Press at 12 tonnes per cm²

Press the grains at 12 tonnes per cm² (ours: discs instead of rods). The patent describes no further firing.

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo per pressatura di dischiStampo per pressatura di dischi
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Strumenti necessari:

ElettromagneteElettromagnete
BussolaBussola

Materiali

3

Strumenti richiesti

14

Questo progetto realizza

Blueprint correlati

Questi blueprint condividono conoscenze — tecniche, materiali o principi

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.