Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Intermedio
30-60 minutes per charge

Istruzioni

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Materiali per questo passaggio:

Minerale di bismuto nativoMinerale di bismuto nativo1 12 cwt per tube charge

Strumenti necessari:

MartelloMartello
Bilancia industriale a piattaformaBilancia industriale a piattaforma
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Materiali per questo passaggio:

Carbone di legnaCarbone di legna1 powdered, in the pots and for the pot fire

Strumenti necessari:

Forno di liquazione del bismutoForno di liquazione del bismuto
Crogiolo di ghisaCrogiolo di ghisa
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Materiali per questo passaggio:

Legna da ardereLegna da ardere1 about 63 cu ft per 20 cwt of ore

Strumenti necessari:

Forno di liquazione del bismutoForno di liquazione del bismuto
Tondino di ferroTondino di ferro
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Strumenti necessari:

Rastrello di ferroRastrello di ferro
Forno di liquazione del bismutoForno di liquazione del bismuto
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Strumenti necessari:

Crogiolo di ghisaCrogiolo di ghisa
Siviera da fonderiaSiviera da fonderia
LingottieraLingottiera

Materiali

3

Strumenti richiesti

8

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...