Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)
Ed

Creato da

Ed

2. novembre 2026FI
11
0
0
0
0

Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)

Barium titanate with 3 mole % nickel stannate is calcined, pressed into small discs and fired hard. Silver is fired onto both faces and a lead soldered to each, giving ceramic disc capacitors of high capacity for their size. Result: discs 3/8 inch across and about 1/10 inch thick with a dielectric constant averaging 2380 and a dissipation factor of 0.58 %. Between 25 and 85 °C the dielectric constant rose at most 17 % and fell at most 7 %. Source: W. W. Coffeen (Metal & Thermit Corp.), US 2,789,061 (1957). Unknown: how the barium titanate, the nickel stannate and the tinned lead wire are made; the patent uses them ready-made. Picture: Wikimedia Commons.
Avanzato
10 days

Istruzioni

1

Weigh and slurry

Weigh 19.32 g of barium titanate and 0.68 g of hydrated nickel stannate (about NiSnO3·2H2O), which is 97 mole % BaTiO3 and 3 mole % NiSnO3. Slurry them with 50 cc of distilled water. The patent prefers 2 to 4 mole % nickel stannate; 1 to 15 % works.

Materiali per questo passaggio:

Titanato di barioTitanato di bario19.32 g
Stannato di nichelStannato di nichel0.68 g

Strumenti necessari:

Acqua distillataAcqua distillata
Bilancia digitale di precisioneBilancia digitale di precisione
Capsula di evaporazioneCapsula di evaporazione
2

Dry, sieve and calcine

Dry the slurry, crush it to pass a 50 mesh screen, moisten it with 5 % of a 2 1/2 % starch solution and press it into one slug. Calcine the slug for one hour at 1600 °F (871 °C). Ours: potato starch, a drying oven, mortar and pestle.

Strumenti necessari:

Fecola di patateFecola di patate
EssiccatoioEssiccatoio
Mortaio e pestelloMortaio e pestello
VaglioVaglio
Pressa idraulicaPressa idraulica
Forno da alta temperaturaForno da alta temperatura
3

Press the discs

Grind the calcine to pass a 325 mesh screen, moisten it again with starch solution, and press small discs 3/8 inch in diameter and about 1/10 inch thick at 20,000 pounds per square inch.

Strumenti necessari:

Mortaio e pestelloMortaio e pestello
Setaccio a maglia fineSetaccio a maglia fine
Fecola di patateFecola di patate
Pressa idraulicaPressa idraulica
Stampo per pressatura di dischiStampo per pressatura di dischi
4

Fire on platinum

Fire the discs on platinum foil at 2400 °F (1316 °C) for one hour. They come out with zero absorption.

Strumenti necessari:

Forno da alta temperaturaForno da alta temperatura
PlatinoPlatino
5

Silver and lead

Paint silver paint on both faces and fire the discs at 1350 °F (732 °C) for one hour. Solder tinned copper lead wires directly to the silver electrodes. Age at least a week before measuring. Ours: a fine brush and a soldering iron.

Materiali per questo passaggio:

Vernice d'argento da cotturaVernice d'argento da cottura1 both faces
Filo di rame stagnatoFilo di rame stagnato2 leads per disc
Filo per saldaturaFilo per saldatura1 a little

Strumenti necessari:

Pennelli a punta finePennelli a punta fine
Forno da alta temperaturaForno da alta temperatura
Saldatore a stagnoSaldatore a stagno

Materiali

5

Strumenti richiesti

14

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...