Coloured Glass Sheets: Beech-Ash Glass Blown into Cylinders and Flattened (Theophilus, tr. Hendrie 1847)

Window glass as the monk Theophilus taught it around 1100: two parts beech ash to one of clean sand, fritted for a night and a day, melted overnight in clay pots, blown into long bladders, opened into cylinders, split and flattened in a second oven, and cooled standing upright. White glass comes first. A pot that turns yellow gives light yellow if heated to the third hour and reddish yellow by the sixth; a pot that turns flesh-coloured gives light purple after two more hours and red purple by the sixth. Source: Theophilus, De Diversis Artibus, Book II, tr. R. Hendrie (1847), pp. 119-129. Picture: p. 127.
Avanzato
2-3 days

Istruzioni

1

Make the beech ash

Cut beech-wood logs and dry them. Burn them together in a clean spot and collect the ashes, taking care that no earth gets mixed in.

Materiali per questo passaggio:

Tronchi di latifoglia (rovere, acero, faggio)Tronchi di latifoglia (rovere, acero, faggio)1 beech

Strumenti necessari:

CazzuolaCazzuola
2

Frit the ash and sand

Mix two parts of ash with one part of sand washed free of earth and stones. Heat it on the upper hearth of the furnace for a night and a day, stirring it with an iron trowel as it warms so that it does not melt into a lump.

Materiali per questo passaggio:

Sabbia di quarzoSabbia di quarzo1 1 part to 2 of ash

Strumenti necessari:

Forno da vetro capace di raggiungere 1100 gradi CelsiusForno da vetro capace di raggiungere 1100 gradi Celsius
CazzuolaCazzuola
3

Make the pots and melt

Grind dry white clay, wet it, beat it hard with wood and make pots wide at the top and narrow below, with a small lip curved inward. Set the dry pots in the glowing furnace, fill them in the evening with the hot frit and feed dry wood all night until the glass is fully melted.

Strumenti necessari:

Caolino in polvereCaolino in polvere
Forno da vetro capace di raggiungere 1100 gradi CelsiusForno da vetro capace di raggiungere 1100 gradi Celsius
Tenaglia da forgiaTenaglia da forgia
CazzuolaCazzuola
4

Blow the cylinders

In the morning gather glass on the iron pipe (two yards long, a thumb thick), blow a little, tap it on a flat stone so it hangs evenly, and blow it into a long bladder. Melt open the far end in the flame and widen it with a piece of wood, break it off the pipe with a wet piece of wood, open the other end the same way, and let a boy carry the cylinder on a stick to the warm cooling oven. This first glass is pure and white.

Strumenti necessari:

Canna da soffiatore di vetroCanna da soffiatore di vetro
Forno da vetro capace di raggiungere 1100 gradi CelsiusForno da vetro capace di raggiungere 1100 gradi Celsius
Forno di ricotturaForno di ricottura
5

Bring out the colours

If a pot turns yellow, heat it to the third hour for light yellow or to the sixth for reddish yellow. If a pot turns tawny like flesh, keep some for flesh tints; heat the rest from the first to the third hour for light purple, from the third to the sixth for a red purple. Blow cylinders from each as before.

Strumenti necessari:

Forno da vetro capace di raggiungere 1100 gradi CelsiusForno da vetro capace di raggiungere 1100 gradi Celsius
Canna da soffiatore di vetroCanna da soffiatore di vetro
6

Split and flatten

When all are made and cooled, fire the flattening oven. Split each cylinder along one side with a hot iron, lay it on the glowing hearth, and when it softens open it with the pincers and a smooth piece of wood and flatten it. Stand the sheets upright against the wall of the warm cooling oven, one next to another. When cold, cut them into pieces for windows.

Strumenti necessari:

Forno da vetro capace di raggiungere 1100 gradi CelsiusForno da vetro capace di raggiungere 1100 gradi Celsius
Tenaglia da forgiaTenaglia da forgia
Forno di ricotturaForno di ricottura

Materiali

2

Strumenti richiesti

6

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...