Extruded Polystyrene Foam: Butylene-Blown Logs 20 Inches Across (McIntire, Dow 1948, Ex. 4)

Extruded polystyrene foam blown with a butylene gas fraction. 300 lb of polystyrene and about 130 lb of the fraction stand two days at 110 °C under 265 psi. Opened again and again, the tower let out foam logs 20 inches across and 20 feet long, weighing only 0.8 lb per cubic foot. Unknown: a source for the butylene fraction, linked to an unknown head. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 4. Picture: the patent's drawing.
Avanzato
3 days

Istruzioni

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materiali per questo passaggio:

PolistirenePolistirene300 libbre

Strumenti necessari:

Reattore a pressioneReattore a pressione
Bilancia a bracciBilancia a bracci
Guanti di gommaGuanti di gomma
2

Add the butylene fraction

Add about 130 lb of a cracked-oil gas fraction that is about 87 % normal butylenes, with some butanes and butadiene, under pressure. Unknown: a source for this fraction. Flammable gas: no flames, strong ventilation.

Materiali per questo passaggio:

Frazione di gas di cracking a butileniFrazione di gas di cracking a butileni130 libbre

Strumenti necessari:

Bombola di gas in pressioneBombola di gas in pressione
Reattore a pressioneReattore a pressione
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
3

Heat two days at 110 °C

Close the tower and heat it at 110 °C for two days. The gauge pressure stays at 265 psi.

Strumenti necessari:

Reattore a pressioneReattore a pressione
Termometro da laboratorioTermometro da laboratorio
4

Let out logs through a 3.25 inch outlet

Open and close the 3.25 inch outlet near the bottom again and again. Each portion swells into a foam log 20 inches across and about 20 feet long, with fine, even, closed cells, weighing 0.8 lb per cubic foot.

Strumenti necessari:

Reattore a pressioneReattore a pressione
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
Guanti di gommaGuanti di gomma
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Strumenti necessari:

Sega da falegnameSega da falegname
Guanti di gommaGuanti di gomma

Materiali

2

Strumenti richiesti

7

Blueprint correlati

Questi blueprint condividono conoscenze — tecniche, materiali o principi

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...