Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)
Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells.
Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Avanzato
3 days
Istruzioni
1
1
Charge the tower with polystyrene
Charge the tower with polystyrene
Charge a high-pressure tower with 300 lb of granular polystyrene.
Materiali per questo passaggio:
Polistirene300 libbreStrumenti necessari:
Reattore a pressione
Bilancia a bracci
Guanti di gomma2
2
Add the propylene fraction
Add the propylene fraction
Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.
Materiali per questo passaggio:
Propilene100 libbreStrumenti necessari:
Bombola di gas in pressione
Reattore a pressione
Occhiali antispruzzo chimico3
3
Stand two days at 40 °C
Stand two days at 40 °C
Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.
Strumenti necessari:
Reattore a pressione
Termometro da laboratorio4
4
Let it out at 50 °C
Let it out at 50 °C
Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.
Strumenti necessari:
Reattore a pressione
Termometro da laboratorio
Occhiali antispruzzo chimico
Guanti di gomma5
5
Saw into boards
Saw into boards
When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).
Strumenti necessari:
Sega da falegname
Guanti di gommaStrumenti richiesti
7- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.