Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 75 °C (McIntire, Dow 1948, Ex. 3, Test 4)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 75 °C (395 psi in the tower), it swelled into a log 18 to 20 inches across, weighing 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
Avanzato
3 days

Istruzioni

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Materiali per questo passaggio:

PolistirenePolistirene300 libbre

Strumenti necessari:

Reattore a pressioneReattore a pressione
Bilancia a bracciBilancia a bracci
Guanti di gommaGuanti di gomma
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Materiali per questo passaggio:

PropilenePropilene100 libbre

Strumenti necessari:

Bombola di gas in pressioneBombola di gas in pressione
Reattore a pressioneReattore a pressione
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Strumenti necessari:

Reattore a pressioneReattore a pressione
Termometro da laboratorioTermometro da laboratorio
4

Let it out at 75 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 75 °C. The pressure is about 395 psi. The gel flows out and swells into a log 18 to 20 inches across, 2.9 lb per cubic foot, with uniform cells finer than at 60 °C. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Strumenti necessari:

Reattore a pressioneReattore a pressione
Termometro da laboratorioTermometro da laboratorio
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
Guanti di gommaGuanti di gomma
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Strumenti necessari:

Sega da falegnameSega da falegname
Guanti di gommaGuanti di gomma

Materiali

2
  • 300 libbre
    Segnaposto
  • 100 libbre
    Segnaposto

Strumenti richiesti

7

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...