Ferric Oxide: Hydroxide Precipitated from Ferric Chloride with Ammonia, Then Heated
Charlie

Creato da

Charlie

21. ottobre 2026DE
0
0
0
0
0

Ferric Oxide: Hydroxide Precipitated from Ferric Chloride with Ammonia, Then Heated

Ferric oxide, Fe2O3, made by way of the hydroxide as Thorpe's Dictionary (1912) gives it. Ferric chloride solution with excess ammonia throws down a bulky, brown, slimy hydroxide, which shrinks a great deal as it dries. Heated, it slowly gives up its water at 320 °C; taken to dull redness it suddenly contracts and glows, and is then much less soluble in acids. The picture: our diagram.
Principiante
1 day

Istruzioni

1

Precipitate with excess ammonia

Add excess ammonia to ferric chloride solution: the hydroxide comes down as a bulky, brown, slimy precipitate. No amounts are given. Ours: stir in a beaker in a fume hood.

Materiali per questo passaggio:

Soluzione di cloruro ferricoSoluzione di cloruro ferrico1 as required

Strumenti necessari:

Soluzione di ammoniaca al 25-28 %Soluzione di ammoniaca al 25-28 %
Becher di vetroBecher di vetro
AgitatoreAgitatore
Cappa aspirante (canalizzata)Cappa aspirante (canalizzata)
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
Guanti di gommaGuanti di gomma
2

Filter, wash and dry (ours)

Ours: filter off the precipitate, wash it with water and dry it; it shrinks a great deal as it dries.

Strumenti necessari:

Carta da filtroCarta da filtro
Imbuto di vetro con gamboImbuto di vetro con gambo
Spruzzetta da laboratorioSpruzzetta da laboratorio
Acqua distillataAcqua distillata
EssiccatoioEssiccatoio
3

Heat to dull redness

Heat the dry hydroxide: it gives up its water slowly at 320 °C. Taken on to dull redness, the anhydrous oxide suddenly contracts and glows brightly. Ours: a porcelain crucible in a muffle furnace.

Strumenti necessari:

Crogiolo con coperchio (porcellana)Crogiolo con coperchio (porcellana)
Forno a muffolaForno a muffola
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore

Materiali

1

Strumenti richiesti

15

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.