Ferrite Toroid Core: Copper-Zinc Ferrite Sintered at 1100 °C, Presintered Twice at 900 °C (Snoek 1948, Ex. I)
Charlie

Creato da

Charlie

28. ottobre 2026DE
5
0
0
0
0

Ferrite Toroid Core: Copper-Zinc Ferrite Sintered at 1100 °C, Presintered Twice at 900 °C (Snoek 1948, Ex. I)

A soft ferrite ring core for coils and transformers: copper, zinc and iron oxides with a little brownstone, presintered twice at 900 °C, pressed into a ring and sintered at 1100 °C in oxygen. Snoek's ring had an initial permeability of 154. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example I and its table. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Avanzato
2 days

Istruzioni

1

Weigh 20 : 30 : 50 mol % and 1 % brownstone

Mix 20 mol % pure copper oxide, 30 mol % pure zinc oxide and 50 mol % pure violet iron oxide, and add 1 % by weight of brownstone (manganese dioxide). Ours, by weight: 13.24 g copper oxide, 20.32 g zinc oxide and 66.44 g iron oxide per 100 g, plus 1 g brownstone. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.

Materiali per questo passaggio:

Ossido di rameOssido di rame13.24 g
Polvere di ossido di zincoPolvere di ossido di zinco20.32 g
Ossido di ferro violettoOssido di ferro violetto66.44 g
Biossido di manganese (pirolusite)Biossido di manganese (pirolusite)1 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Mascherina antipolvereMascherina antipolvere
2

Grind half an hour in an iron ball mill

Grind the mixture for half an hour in a mill with iron balls.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Mascherina antipolvereMascherina antipolvere
3

Presinter at 900 °C for 2 hours in oxygen

Heat the ground powder to 900 °C for 2 hours in oxygen and let it cool.

Strumenti necessari:

Forno a tuboForno a tubo
OssigenoOssigeno
Bombola di gas in pressioneBombola di gas in pressione
PirometroPirometro
Crogiolo con coperchio (porcellana)Crogiolo con coperchio (porcellana)
Guanti resistenti al caloreGuanti resistenti al calore
4

Grind and presinter at 900 °C again (2 of 2)

Grind the powder, then heat it once more to 900 °C in oxygen. Snoek gives no times for the repeats.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Forno a tuboForno a tubo
OssigenoOssigeno
Bombola di gas in pressioneBombola di gas in pressione
Crogiolo con coperchio (porcellana)Crogiolo con coperchio (porcellana)
Guanti resistenti al caloreGuanti resistenti al calore
Mascherina antipolvereMascherina antipolvere
5

Grind 2 hours with iron balls

Grind it for 2 hours in a disintegrator with iron balls.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Mascherina antipolvereMascherina antipolvere
6

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo di pressatura ad anelloStampo di pressatura ad anello
Mascherina antipolvereMascherina antipolvere
7

Sinter at 1100 °C in oxygen, cool 5–10 °C a minute

Sinter the ring at 1100 °C in a current of oxygen. Example I heats for 1 hour and cools in the oxygen at 5 to 10 °C per minute. Snoek's ring had an initial permeability of 154, measured at room temperature at 2 kHz.

Strumenti necessari:

Forno a tuboForno a tubo
OssigenoOssigeno
Bombola di gas in pressioneBombola di gas in pressione
PirometroPirometro
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore

Materiali

4

Strumenti richiesti

12

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...