Ferrite Toroid Core: Copper-Zinc Ferrite by the Wet Process, Precipitated with Caustic Soda (Snoek 1948)

Snoek's copper-zinc ferrite made the wet way: copper, zinc and iron salts thrown down together with hot caustic soda, so the particles are very fine and pure. The washed deposit is pre-heated, pressed into a ring and fired in oxygen, with a 30-hour hold at 600 °C. His core reached an initial permeability of 500. Source: J. L. Snoek, US 2,452,529 (Philips, 1948), Example II, wet process. Picture: our diagram.
Avanzato
3 days

Istruzioni

1

Dissolve the copper, zinc and iron salts

Make 1 litre of a purified solution of 0.2 mol copper sulphate, 0.3 mol zinc sulphate and 1 mol iron nitrate. Ours: 49.94 g copper sulphate pentahydrate; weigh the zinc sulphate and ferric nitrate for the hydrate you have.

Materiali per questo passaggio:

Solfato di rame pentaidrato (CuSO4·5H2O)Solfato di rame pentaidrato (CuSO4·5H2O)49.94 g
Solfato di zincoSolfato di zinco0.3 mol
Nitrato ferricoNitrato ferrico1 mol
Acqua distillataAcqua distillata1 l

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Becher in borosilicatoBecher in borosilicato
Guanti di gommaGuanti di gomma
2

Precipitate hot with 9 M caustic soda

Heat the solution and precipitate it with 0.5 litre of 9 molar caustic soda. Ours: 180 g sodium hydroxide in water to 0.5 litre. Strong alkali: goggles and gloves.

Materiali per questo passaggio:

Idrossido di sodio — grado laboratorioIdrossido di sodio — grado laboratorio180 g

Strumenti necessari:

Becher in borosilicatoBecher in borosilicato
Piastra riscaldantePiastra riscaldante
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
Guanti di gommaGuanti di gomma
3

Wash, dry and pre-heat at 700 °C

Wash out the deposit, dry it, and pre-heat it at 700 °C so it moulds better.

Strumenti necessari:

Carta da filtroCarta da filtro
Acqua distillataAcqua distillata
EssiccatoioEssiccatoio
Forno a tuboForno a tubo
Crogiolo con coperchio (porcellana)Crogiolo con coperchio (porcellana)
Guanti resistenti al caloreGuanti resistenti al calore
4

Mould a ring at 4 tons per cm²

Mould the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm section.

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo di pressatura ad anelloStampo di pressatura ad anello
Mascherina antipolvereMascherina antipolvere
5

Heat 3 hours at 900 °C, cool to 600 °C, hold 30 hours

Heat the ring for about 3 hours at 900 °C, cool it to 600 °C at 5 °C per minute, hold it there for 30 hours and let it cool to room temperature, all in a current of oxygen. Snoek's core: initial permeability 500.

Strumenti necessari:

Forno a tuboForno a tubo
OssigenoOssigeno
Bombola di gas in pressioneBombola di gas in pressione
PirometroPirometro
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore

Materiali

5

Strumenti richiesti

18

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...