Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)
Charlie

Creato da

Charlie

28. ottobre 2026DE
6
0
0
0
0

Ferrite Toroid Core: Magnesium-Zinc Ferrite, One-Day Grind, 1400 °C (Snoek 1948, Ex. II)

A soft ferrite ring core of magnesium-zinc ferrite: magnesia, zinc oxide and iron oxide ground for a whole day, pressed into a ring and fired at 1400 °C in oxygen. Snoek's ring had an initial permeability of 670 and a Curie point near 100 °C. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example II. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Avanzato
2 days

Istruzioni

1

Weigh 25.5 : 25.5 : 49 mol %

Mix 25½ mol % pure magnesia, 25½ mol % pure zinc oxide and 49 mol % pure violet iron oxide. Ours, by weight: 9.4 g magnesium oxide, 18.99 g zinc oxide and 71.61 g iron oxide per 100 g. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.

Materiali per questo passaggio:

Ossido di magnesioOssido di magnesio9.4 g
Polvere di ossido di zincoPolvere di ossido di zinco18.99 g
Ossido di ferro violettoOssido di ferro violetto71.61 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Mascherina antipolvereMascherina antipolvere
2

Grind for one day in an iron ball mill

Grind the mixture for one day in a mill with iron balls.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Mascherina antipolvereMascherina antipolvere
3

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo di pressatura ad anelloStampo di pressatura ad anello
Mascherina antipolvereMascherina antipolvere
4

Fire 1 hour at 1400 °C, cool slowly in oxygen

Heat the ring in oxygen for 1 hour at 1400 °C, then cool it slowly in oxygen. Snoek's ring had an initial permeability of 670 at room temperature and 2 kHz.

Strumenti necessari:

Forno a tuboForno a tubo
OssigenoOssigeno
Bombola di gas in pressioneBombola di gas in pressione
PirometroPirometro
Tenaglia per crogioloTenaglia per crogiolo
Guanti resistenti al caloreGuanti resistenti al calore

Materiali

3

Strumenti richiesti

11

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...