Fired Silver Paint: Precipitated Silver and Flux in Polyvinyl Alcohol with Ammonia (Gray, Erie Resistor 1954, Ex. 1)

A paint for putting silver electrodes on ceramic, glass or mica. Fine silver powder and a little ceramic flux are held in polyvinyl alcohol dissolved in water, with a trace of ammonia to make the wet paint conduct. So a capacitor can be measured while it is being painted. On firing, the silver becomes a film held on by the flux. The silver settles, so stir while painting. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 1. Not given: how the silver was precipitated, which flux, the form of the ammonia, and the firing heat. Ours: precipitated silver made by reducing silver chloride with zinc, bismuth subnitrate as the flux (one Gray names), and strong ammonia water. Picture drawn by Youblob.
Principiante
1 day

Istruzioni

1

Dissolve 4 g polyvinyl alcohol in the water

For 100 g of paint: dissolve 4 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 35 to 44 g. Warming is ours.

Materiali per questo passaggio:

Alcol polivinilico in polvereAlcol polivinilico in polvere4 g
Acqua distillataAcqua distillata1 as required

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Becher in borosilicatoBecher in borosilicato
Piastra riscaldantePiastra riscaldante
Bacchetta in vetro borosilicatoBacchetta in vetro borosilicato
2

Grind in 50 g precipitated silver and the flux

Grind 50 g precipitated silver and 2 to 10 g ceramic flux into the solution until smooth. Gray allows some silver chloride left in the silver. Ours: silver from the zinc route, and bismuth subnitrate, one of the fluxes Gray names. The right amount of flux depends on the ceramic.

Materiali per questo passaggio:

Argento precipitatoArgento precipitato50 g
Subnitrato di bismutoSubnitrato di bismuto1 as required

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Mortaio e pestelloMortaio e pestello
Guanti in nitrileGuanti in nitrile
3

Add 0.2 to 1 % ammonia

Stir in ammonia, 0.2 to 1 % of the paint. It evaporates from the film but makes the wet paint conduct. Ours: added as strong ammonia water. Sharp fumes: work in air, goggles.

Materiali per questo passaggio:

Soluzione di ammoniaca al 25-28 %Soluzione di ammoniaca al 25-28 %1 as required

Strumenti necessari:

Bacchetta in vetro borosilicatoBacchetta in vetro borosilicato
Occhiali antispruzzo chimicoOcchiali antispruzzo chimico
Guanti in nitrileGuanti in nitrile
4

Stir while painting

The silver in this paint settles, so stir it while it is being applied.

Strumenti necessari:

Bacchetta in vetro borosilicatoBacchetta in vetro borosilicato

Materiali

5

Strumenti richiesti

7

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...