Fired Silver Paint: Silver Oxide Paint with Silver Nitrate Added Just Before Use (Gray, Erie Resistor 1954, Ex. 5)

A paint for putting silver electrodes on ceramic, glass or mica. Silver oxide and a little ceramic flux are held in polyvinyl alcohol dissolved in water. The wet paint conducts electricity, so a capacitor can be measured while it is being painted. On firing, the silver oxide turns into a silver film held on by the flux. This version adds up to 3 % silver nitrate just before use, which makes the wet paint conduct better. Source: Robert B. Gray, US 2,695,275 (Erie Resistor, 1954), Example 5. Not given: which flux, and the firing heat. Bismuth subnitrate, one of the fluxes Gray names, is ours. Picture drawn by Youblob.
Principiante
1 day

Istruzioni

1

Dissolve 2 g polyvinyl alcohol in the water

For 100 g of paint: dissolve 2 g polyvinyl alcohol in the water, warming it to help it dissolve. The water is the balance, about 34 to 44 g. Warming is ours.

Materiali per questo passaggio:

Alcol polivinilico in polvereAlcol polivinilico in polvere2 g
Acqua distillataAcqua distillata1 as required

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Becher in borosilicatoBecher in borosilicato
Piastra riscaldantePiastra riscaldante
Bacchetta in vetro borosilicatoBacchetta in vetro borosilicato
2

Grind in silver oxide and flux

Grind 50 g precipitated silver oxide and 2 to 10 g ceramic flux into the solution until smooth. Gray gives the flux only as a class; ours: bismuth subnitrate, one of the common fluxes he names. The right amount depends on the ceramic it will be fired onto.

Materiali per questo passaggio:

Ossido d'argentoOssido d'argento50 g
Subnitrato di bismutoSubnitrato di bismuto1 as required

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Mortaio e pestelloMortaio e pestello
Guanti in nitrileGuanti in nitrile
3

Add 2 to 4 g alcohol against foam

Stir in 2 to 4 g ethyl alcohol. It stops the polyvinyl alcohol from foaming.

Materiali per questo passaggio:

Etanolo per laboratorio, 95 %Etanolo per laboratorio, 95 %1 as required

Strumenti necessari:

Bacchetta in vetro borosilicatoBacchetta in vetro borosilicato
4

Add up to 3 g silver nitrate just before use

Just before painting, stir in 0 to 3 g silver nitrate. With polyvinyl alcohol it must go in immediately before use, or it breaks the binder down. Silver nitrate stains and burns skin: gloves.

Materiali per questo passaggio:

Nitrato d'argentoNitrato d'argento1 as required

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Bacchetta in vetro borosilicatoBacchetta in vetro borosilicato
Guanti in nitrileGuanti in nitrile

Materiali

6

Strumenti richiesti

6

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...