Forged Ball-Peen Hammer
A 2-pound ball-peen hammer forged from 1½-inch square tool steel; a 6½-inch bar gives two heads. The eye is punched and drifted, the body fullered and rounded so it tapers both ways from a thick centre, then the face is drawn out and swaged and the ball peen rounded in a bottom swage. Both ends are hardened by dipping them in turn, with water dripping on the face, and tempered from the heat held around the eye: dark brown for the face, brown or purple for the peen. The eye cools last, which keeps it tough.
Avanzato
4–6 hours
Istruzioni
1
1
Mark and flatten
Mark and flatten
Mark the bar with a chisel and centre punch. Flatten the end before punching, or the hole grows too large.
Materiali per questo passaggio:
Barra quadra di acciaio per utensili1 pezzoStrumenti necessari:
Bulino da centro
Tagliolo a caldo
Forgia da fabbro
Incudine
Mazza
Tenaglie da fabbro2
2
Punch and drift the eye
Punch and drift the eye
Punch the eye at the centre-punch mark, drive in a drift and hammer the bulged sides straight.
Strumenti necessari:
Punzone a caldo
Spina allargafori
Martello da fucina3
3
Shape the body
Shape the body
Rough out the shape with top and bottom fullers, then round the body at the anvil's rounded edge with a top fuller and set hammer, thicker at the centre than at the ends.
Strumenti necessari:
Fuller (ferro da scanalare)
Spianatoio a spigolo (set hammer)4
4
Face and peen
Face and peen
Cut the head from the bar from four sides for a square end. Draw out the face, swage it and trim it with a hot chisel; then cut the peen to length, cut off its corners and round it in a bottom swage. Drive the drift through from both sides to taper the eye.
Strumenti necessari:
Tagliolo a caldo
Stampo inferiore
Spina allargafori5
5
Grind
Grind
Grind both ends, rounding the edges of the face slightly so it does not mark hot work.
Strumenti necessari:
Smerigliatrice da banco6
6
Harden and temper
Harden and temper
Heat the whole head slowly to the hardening heat and hold it by a tong jaw in the eye. Lower about 1½ inches of the face into water, then harden the peen the same way while water drips on the face, keeping the eye hot. Polish the ends; take the face to dark brown and the peen to brown or purple, then dip the ends alternately so the eye cools slowly.
Strumenti necessari:
Forgia da fabbro
Tinozza di tempra
Tenaglie da fabbro
Tela smeriglio7
7
Handle
Handle
Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.
Materiali per questo passaggio:
Listello di legno duro per manici1 pezzo
Zeppa di legno duro1 pezzo
Olio di lino10 mlStrumenti necessari:
Pialletto a due manici
Sega a due mani
Morsa da bancoMateriali
4- Segnaposto
- Segnaposto
- 1 pezzoSegnaposto
- 10 mlSegnaposto
Strumenti richiesti
18- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.