Forged Hunting Axe (Hatchet)
A small one-handed axe forged from a 7/8 × 2-inch bar of good tool steel, best made by two people; a 6¾-inch bar gives two heads. The eye, about 9/16 × 1½ inches, is punched at a yellow heat with an eye punch and opened with drifts, the blade drawn out to a 3-inch edge and the head cut to length. The axe is annealed in lime or ashes, ground and buffed, then hardened from the hardening heat in tepid water and tempered by two hot iron bars laid on either side at the centre: dark purple for the blade, blue for the head.
Avanzato
4–6 hours
Istruzioni
1
1
Mark and punch the eye
Mark and punch the eye
Mark the stock with chisel and centre punch. At a yellow heat, punch the eye with the narrow edge of the punch toward the blade; lift the punch after each blow to check it runs straight and to let it cool; a little fine coal in the hole stops it sticking. Punch nearly through, then finish from the other side.
Materiali per questo passaggio:
Barra piatta di acciaio per utensili1 pezzoStrumenti necessari:
Bulino da centro
Forgia da fabbro
Incudine
Punzone a caldo
Mazza
Tenaglie da fabbro2
2
Drift and draw out
Drift and draw out
Drive in a tool-steel drift, hammer the bulges down to the bar's size and smooth with a flatter; take the drift out before each reheat. Use two drifts, the first 3/8 inch narrower. Draw out the blade, driving the drift back in as the eye stretches so no cold shut forms.
Strumenti necessari:
Spina allargafori
Spianatoio da fabbro
Maglio a camme3
3
Shape and trim
Shape and trim
Shape the blade with a heavy hammer and flatter and form its edge. Cut the head from the bar, draw it to size, cut it to length, then trim the blade to shape.
Strumenti necessari:
Martello da fucina
Spianatoio da fabbro
Tagliolo a caldo4
4
Anneal and grind
Anneal and grind
Heat to a full red and anneal in lime or ashes. When cold, grind on an emery wheel and finish on a buffing wheel.
Strumenti necessari:
Forgia da fabbro
Smerigliatrice da banco5
5
Harden and temper
Harden and temper
Heat very slowly to the hardening heat and cool in tepid water. Draw the temper with two hot iron bars laid on either side at the centre; when the blade is dark purple and the head blue, cool quickly in water.
Strumenti necessari:
Forgia da fabbro
Tinozza di tempra
Tenaglie da fabbro6
6
Handle
Handle
Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.
Materiali per questo passaggio:
Listello di legno duro per manici1 pezzo
Zeppa di legno duro1 pezzo
Olio di lino10 mlStrumenti necessari:
Pialletto a due manici
Sega a due mani
Morsa da bancoMateriali
4- Segnaposto
- Segnaposto
- 1 pezzoSegnaposto
- 10 mlSegnaposto
Strumenti richiesti
16- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
- Segnaposto
Questo progetto realizza
Blueprint correlati
Questi blueprint condividono conoscenze — tecniche, materiali o principi
CC0 Pubblico dominio
Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.
Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.