Rasps: Teeth Raised One at a Time with a Pointed Punch
Forge

Creato da

Forge

11. ottobre 2026NO
32
0
0
0
0

Rasps: Teeth Raised One at a Time with a Pointed Punch

A rasp is a coarse file whose teeth stand separately instead of in continuous rows. Each tooth is raised by driving a pointed punch into the face of the blank at uniform distances. Because the teeth stand apart, a rasp clogs less than a cut file on soft material such as wood or a horse's hoof. The blank is forged, annealed and ground like a file blank, and the finished rasp is hardened like a file: coated against scale, brought to a dull red heat and plunged into water, with the tang tempered so it will not snap. Machine-made rasps have uniformly stamped teeth, which line up row behind row and leave deeper marks; slightly uneven hand-cut teeth avoid this.
Avanzato
2 days (annealing overnight)

Istruzioni

1

Forge the blank

Forge the steel to a tapered bar, flat, round or half-round, with a narrow pointed tang at one end.

Materiali per questo passaggio:

Billetta di acciaio ad alto carbonioBilletta di acciaio ad alto carbonio0.5 kg

Strumenti necessari:

Forgia da fabbroForgia da fabbro
IncudineIncudine
Martello da fucinaMartello da fucina
Tenaglia da forgiaTenaglia da forgia
2

Anneal and grind

Anneal the blank soft so the teeth can be raised, then grind the faces to a smooth, clear surface.

Strumenti necessari:

Forgia da fabbroForgia da fabbro
Mola ad acquaMola ad acqua
3

Punch the teeth

Drive the pointed punch into the face with the hammer at uniform distances, raising one separate tooth at each blow. Turn the rasp over on a soft metal plate to work the other face without crushing the finished teeth.

Strumenti necessari:

Punzone per raspePunzone per raspe
Martello da fucinaMartello da fucina
IncudineIncudine
Lastra di peltroLastra di peltro
4

Harden

Coat the toothed surface thickly with a salt composition against scaling, raise the rasp to a dull red heat in a clear coke fire and plunge it upright into water. If it bends, straighten it across a fulcrum before it is fully cold.

Materiali per questo passaggio:

SaleSale1 kg
Coke metallurgicoCoke metallurgico1 as required

Strumenti necessari:

Forgia da fabbroForgia da fabbro
SecchioSecchio
Tenaglia da forgiaTenaglia da forgia
5

Temper the tang and clean

Temper the tang by dipping it in molten lead so it will not snap. Scour and wash off every trace of salt, then brush the rasp with oil.

Strumenti necessari:

Bagno di piombo fusoBagno di piombo fuso
Tenaglia da forgiaTenaglia da forgia

Materiali

3

Strumenti richiesti

9

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...