Nylon 66 Pellets: Nylon Salt Polymerised in an Autoclave, Carothers 1938

Nylon salt heated to 288 °C under oxygen-free nitrogen gives off water and joins into long chains of nylon 66 (Carothers, du Pont, US 2,130,948, 1938: two moles of salt in a silver-lined autoclave). A pinch of extra adipic acid keeps the melt's viscosity steady. The polymer is then extruded and cut into pellets. The picture: our drawing of the autoclave and the pellet line.
Avanzato
A day

Istruzioni

1

Charge the autoclave

Put two moles of nylon salt (525 g) and 0.02 mole of adipic acid (2.9 g) in a two-litre silver-lined autoclave with a stainless stirrer and a reflux condenser leading to a receiver.

Materiali per questo passaggio:

Sale di nylonSale di nylon525 g
Acido adipicoAcido adipico2.9 g

Strumenti necessari:

Reattore a pressioneReattore a pressione
Serpentina del condensatoreSerpentina del condensatore
Bilancia digitale da cucinaBilancia digitale da cucina
2

Drive out the air

Evacuate, fill with nitrogen, evacuate again, then apply 80 lb/in² of nitrogen. Use nitrogen free of oxygen; oxygen spoils the polymer.

Strumenti necessari:

Pompa per vuotoPompa per vuoto
AzotoAzoto
ManometroManometro
3

Heat to 288 °C

Start the stirrer and heat to 288 °C over 1.5 hours.

Strumenti necessari:

Reattore a pressioneReattore a pressione
Termocoppia con lettoreTermocoppia con lettore
4

Let the water off

Bring the pressure down to atmospheric over half an hour and keep heating and stirring 2.5 hours. Then pull to 200 mm absolute for a few minutes.

Strumenti necessari:

Reattore a pressioneReattore a pressione
Pompa per vuotoPompa per vuoto
ManometroManometro
Termocoppia con lettoreTermocoppia con lettore
5

Cool and take out

Cool. The polymer comes out as a white solid cake that melts at about 263 °C.

Strumenti necessari:

Reattore a pressioneReattore a pressione
6

Pelletise

Break up the cake (our step), melt it in the extruder, draw the strand and cut it into pellets.

Strumenti necessari:

Estrusore per plasticaEstrusore per plastica
Matrice di estrusioneMatrice di estrusione
7

Grams and pressures

Caricamento del notebook Jupyter…

Materiali

2

Strumenti richiesti

9

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...