Precipitated Silica: Hot Water Glass Carbonated, Then Acidified to pH 6.75 (Allen 1957)

Bubble carbon dioxide through hot dilute water glass and the silica comes down as an extremely fine white powder rather than a gel. Edward Allen of Columbia-Southern made it this way as a white reinforcing filler for rubber; this follows his Example XI, which gave a powder of 148 m² per gram. Source: E. M. Allen (Columbia-Southern), US 2,805,955 (1957), Example XI. The percentages are our arithmetic; the filter, mill and indicator are ours. Picture drawn by Youblob.
Intermedio
2 days

Istruzioni

1

Dilute the water glass

Take 12,850 g of sodium silicate solution holding 976 g Na2O and 3115 g SiO2 (7.6 % and 24.2 %, a silica to soda ratio of 3.19 by weight; our arithmetic). Dilute it with water to 48 litres in a stirred kettle with a heating coil and thermometer, and heat to 95 °C.

Materiali per questo passaggio:

Vetro solubile (soluzione di silicato di sodio)Vetro solubile (soluzione di silicato di sodio)12850 g
AcquaAcqua1 as required

Strumenti necessari:

Reattore a pressioneReattore a pressione
AgitatoreAgitatore
TermometroTermometro
Bilancia a bracciBilancia a bracci
2

Carbonate for an hour

Bubble in pure carbon dioxide fast enough to add the theoretical amount in about 30 minutes, and keep going at that rate for about 1 hour. The slurry ends at pH 9.85.

Strumenti necessari:

Anidride carbonica gassosaAnidride carbonica gassosa
Reattore a pressioneReattore a pressione
AgitatoreAgitatore
TermometroTermometro
Cartina indicatrice di pHCartina indicatrice di pH
3

Filter and wash

Filter the slurry and wash the cake twice with hot water.

Materiali per questo passaggio:

AcquaAcqua1 as required

Strumenti necessari:

Imbuto di Büchner (porcellana)Imbuto di Büchner (porcellana)
Carta da filtroCarta da filtro
4

Acidify to pH 6.75

Stir the cake back into water and bring it to pH 6.75 with 400 ml of 3.5 N hydrochloric acid.

Materiali per questo passaggio:

AcquaAcqua1 as required

Strumenti necessari:

Acido cloridricoAcido cloridrico
Recipiente di vetroRecipiente di vetro
AgitatoreAgitatore
Cartina indicatrice di pHCartina indicatrice di pH
5

Wash out the chloride

Filter again and wash the cake with hot water until it is nearly free of chloride.

Materiali per questo passaggio:

AcquaAcqua1 as required

Strumenti necessari:

Imbuto di Büchner (porcellana)Imbuto di Büchner (porcellana)
Carta da filtroCarta da filtro
6

Dry at 105 °C and grind

Dry it at 105 °C in a fan oven and grind it to a fine powder. Allen's had a pH of 8.2, 0.61 % sodium and a surface area of 148 m² per gram.

Strumenti necessari:

EssiccatoioEssiccatoio
Mortaio e pestelloMortaio e pestello
Barattoli di vetro con coperchioBarattoli di vetro con coperchio

Materiali

2

Strumenti richiesti

13

Questo progetto realizza

Blueprint correlati

Questi blueprint condividono conoscenze — tecniche, materiali o principi

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...