PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered
English
Emma

Creato da

Emma

26. ottobre 2026SE
13
0
0
0
0

PTFE Thread Seal Tape: Paste-Extruded, Calendered, Never Sintered

The white tape wound on pipe threads is PTFE that has never been melted. Fine PTFE powder is mixed with a lubricant, pressed into a slug, squeezed through a slit die by a ram, rolled thin between two rolls, and dried. Kept below the sintering heat (about 350 °C) it stays soft and conforms to the thread (process: US 5,415,939, 1995). The targets and tests are those of the Indian standard IS 14643 (from BS 4375): no fillers, at most 0.1 % lubricant left, usually 12 mm wide and 0.075 mm thick. The lubricant (naphtha) and the slitter are ours. The picture: Fig. 1a of the patent.
Avanzato
1 day

Istruzioni

1

Wet the powder

Mix fine (dispersion-made) virgin PTFE powder with a lubricant that can be driven off completely. Granular PTFE will not paste-extrude. No fillers. Ours: naphtha, as required.

Materiali per questo passaggio:

Polvere fine di PTFEPolvere fine di PTFE1 batch

Strumenti necessari:

NaftaNafta
2

Press a preform

Compact the wet powder into a cylindrical preform in a mould with a plunger.

Strumenti necessari:

Stampo a compressioneStampo a compressione
Pressa idraulicaPressa idraulica
3

Ram-extrude a flat tape

Put the preform in the extrusion press. The plunger pushes it out through a slit die as a thick flat tape.

Strumenti necessari:

Pressa idraulica per estrusionePressa idraulica per estrusione
4

Calender it thin

Pass the tape between two counter-rotating rolls to a thin tape, aiming at about 0.075 mm.

Strumenti necessari:

LaminatoioLaminatoio
MicrometroMicrometro
5

Dry off the lubricant

Dry the tape until the lubricant is gone. Keep it well below the sintering heat (about 350 °C): sintered tape is stiff and will not seal.

Strumenti necessari:

EssiccatoioEssiccatoio
6

Slit and spool

Slit it to width, usually 12 mm (±0.5 mm), and wind it on spools.

Strumenti necessari:

Taglierina-ribobinatriceTaglierina-ribobinatrice
7

Check the tape

It must look white, with no visible specks or torn edges. Measure the thickness at five points along a sample; each must be within 10 % of their mean.

Strumenti necessari:

MicrometroMicrometro
8

Test the residual lubricant

Weigh about 15 g of tape. Extract it in a Soxhlet with petroleum spirit (40-60 °C) for at least 4 h, dry it at 100 °C, then heat it at 300 °C for 6 h, cool and weigh. The loss must be 0.1 % or less.

Strumenti necessari:

Estrattore SoxhletEstrattore Soxhlet
Etere di petrolioEtere di petrolio
EssiccatoioEssiccatoio
Crogiolo d'acciaioCrogiolo d'acciaio
Camera di essiccazione (piccola)Camera di essiccazione (piccola)
Bilancia digitale di precisioneBilancia digitale di precisione
9

Wrap a thread

Wind tape round an R 1/2 taper pipe thread with 50 % overlap, two layers deep, just tight enough to take the thread form. It must hold the form, not break, and its end must stay put.

Strumenti necessari:

Raccordo filettato per tubazioniRaccordo filettato per tubazioni

Materiali

1

Strumenti richiesti

14

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...