Rubber Stoppers: Pará Rubber with Ceresine, Moulded and Cured (Heil & Esch 1909)

Laboratory rubber stoppers from a 1909 rubber factory's book of mixings: Pará rubber with ceresine wax, sulphur and magnesia, run out as a cord, cut to weight, pressed into moulds and cured. Source: Heil & Esch, The Manufacture of Rubber Goods (1909), mixing No. 34 (p. 108) and the stopper method (p. 135). They give no cure time or temperature. Using smoked ball rubber as their Pará, and the mill, clamps and steam vessel, are ours. Picture: their page of mixings.
Intermedio
1 day

Istruzioni

1

Weigh mixing No. 34

Weigh out 10,000 g Pará rubber, 2,000 g ceresine, 1,000 g sulphur and 100 g calcined magnesia (magnesia usta).

Materiali per questo passaggio:

Palla di gomma affumicataPalla di gomma affumicata10000 g
Cera ceresinaCera ceresina2000 g
Zolfo in polvereZolfo in polvere1000 g
Ossido di magnesioOssido di magnesio100 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
2

Mix on the rolls

Work the rubber on the mixing rolls and work the ceresine, sulphur and magnesia into it until the mixing is even.

Strumenti necessari:

Mescolatore a due cilindri per gommaMescolatore a due cilindri per gomma
3

Run a cord on the tube machine

Run the mixing through the tube machine as a cord of a size to suit the stoppers. It must be free from air bubbles, or the stoppers will be faulty after curing.

Strumenti necessari:

Trafila per gommaTrafila per gomma
4

Cut pieces to weight

Cut the cord into pieces of the exact weight of one stopper plus 2 or 3 per cent, for what squeezes out of the mould.

Strumenti necessari:

Taglierino di precisioneTaglierino di precisione
Bilancia a bracciBilancia a bracci
5

Press into moulds and clamp

Press each piece into a mould and clamp the small moulds very tightly in iron clips.

Strumenti necessari:

Stampo di vulcanizzazioneStampo di vulcanizzazione
Morsetto a CMorsetto a C
6

Cure in steam

Cure the clamped moulds in a steam heater (Heil & Esch also name the sulphur bath). They give no time or temperature for stoppers; then open the moulds and take out the stoppers.

Strumenti necessari:

Autoclave da bancoAutoclave da banco
Stampo di vulcanizzazioneStampo di vulcanizzazione

Materiali

4

Strumenti richiesti

7

Questo progetto realizza

Blueprint correlati

Questi blueprint condividono conoscenze — tecniche, materiali o principi

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...