Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)
Charlie

Creato da

Charlie

28. ottobre 2026DE
4
0
0
0
0

Strontium-Calcium Ferrite Disc Magnet: 0.08 mol SrCO3 and 0.02 mol CaCO3, 1280 °C (Went, Philips 1956, Ex. 23)

A strontium ferrite with a fifth of the strontium replaced by calcium: 0.08 mol strontium carbonate and 0.02 mol calcium carbonate to 0.6 mol iron oxide, ground, dried, formed and passed through a 1280 °C furnace in 10 minutes. Went's rod held 2,320 gauss with a coercive force of 1,395 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 23. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Avanzato
2 days

Istruzioni

1

Weigh the carbonates and iron oxide

Weigh 11.81 g strontium carbonate (0.08 mol), 2.002 g calcium carbonate (0.02 mol), 95.55 g ferric oxide (0.6 mol).

Materiali per questo passaggio:

Carbonato di stronzioCarbonato di stronzio11.81 g
Carbonato di calcio (bianco di Spagna)Carbonato di calcio (bianco di Spagna)2.002 g
Ossido ferricoOssido ferrico95.55 g

Strumenti necessari:

Bilancia a bracciBilancia a bracci
Respiratore P100Respiratore P100
2

Mill with alcohol 4 hours, dry

As in Examples 18 to 21: grind the mixture with alcohol in a ball mill for 4 hours, then dry it.

Strumenti necessari:

Mulino a sfere di ferroMulino a sfere di ferro
Etanolo per laboratorio, 95 %Etanolo per laboratorio, 95 %
EssiccatoioEssiccatoio
3

Press at 1.5 t/cm²

Example 23 does not say whether the 1000 °C presinter of Examples 18 to 21 is used. Press the dry powder at 1.5 tonnes per cm² (ours: discs instead of a rod).

Strumenti necessari:

Pressa idraulicaPressa idraulica
Stampo per pressatura di dischiStampo per pressatura di dischi
4

Pass through a 1280 °C zone in 10 minutes

Sinter at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Strumenti necessari:

Forno a tuboForno a tubo
Guanti resistenti al caloreGuanti resistenti al calore
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Strumenti necessari:

ElettromagneteElettromagnete
BussolaBussola

Materiali

3

Strumenti richiesti

11

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...