ARTE
BELLEZZA E BENESSERE
MESTIERE
CULTURA E STORIA
DIVERTIMENTO
AMBIENTE
CIBO E BEVANDE
INGEGNERIA INVERSA
SCIENZE
SPORT
TECNOLOGIA
INDOSSABILI
Tinned Copper Saucepan, Raised from Sheet and Riveted
Forge

Creato da

Forge

14. ottobre 2026NO
22
0
0
0
0

Tinned Copper Saucepan, Raised from Sheet and Riveted

A copper saucepan heats evenly; lined with tin, it keeps the copper away from the food. Raise a copper disc into a pan over the stake, anneal it whenever it stiffens, rivet on an iron handle, then tin the inside as Andrew Ure (1839) describes: scour, heat, rub with sal ammoniac, melt tin with rosin on it and wipe it over with tow. The picture: copper saucepans with riveted iron handles in the kitchen of Bourbilly Castle, Burgundy.
Avanzato
Two days

Istruzioni

1

Cut and raise

Cut a disc from copper sheet. Hammer it down into a hollow in a wooden block, then raise the sides in courses over the anvil horn with the raising hammer, turning the work. Anneal to a dull red and quench whenever it stiffens.

Materiali per questo passaggio:

Lamiera di rameLamiera di rame1 pezzo
AcquaAcqua10 litri

Strumenti necessari:

Cesoie da lattoniereCesoie da lattoniere
Martello da imbutireMartello da imbutire
Mazzuolo di legnoMazzuolo di legno
IncudineIncudine
Cannello a propanoCannello a propano
Tinozza di tempraTinozza di tempra
Guanti resistenti al caloreGuanti resistenti al calore
2

Planish and trim

Planish the pan smooth with light overlapping blows, trim the rim level and roll it slightly outward.

Strumenti necessari:

Martello da imbutireMartello da imbutire
IncudineIncudine
Cesoie da lattoniereCesoie da lattoniere
3

Handle

Forge a flat-ended handle from wrought iron rod, drill it and the pan wall, and rivet it on with copper rivets.

Materiali per questo passaggio:

Tondino di ferro battutoTondino di ferro battuto0.3 m
Rivetti di rameRivetti di rame3 pezzi
Carbone di legnaCarbone di legna1 as required

Strumenti necessari:

Forgia da fabbroForgia da fabbro
Martello a penna trasversaleMartello a penna trasversale
Tenaglie da fabbroTenaglie da fabbro
Trapano a manoTrapano a mano
4

Tin the inside

Scour the inside bright with sandstone. Heat the pan and rub it with sal ammoniac until perfectly clean. Put tin and a little pounded rosin in, keep it hot enough to melt the tin, and spread it thinly over the whole inside with a pad of tow. Work outdoors: the sal ammoniac fumes.

Materiali per questo passaggio:

Lingotto di stagnoLingotto di stagno10 g
Cloruro di ammonio (NH₄Cl)Cloruro di ammonio (NH₄Cl)10 g
Colofonia di pinoColofonia di pino5 g
Stoppa di linoStoppa di lino1 pezzo

Strumenti necessari:

Cannello a propanoCannello a propano
Guanti resistenti al caloreGuanti resistenti al calore
Mascherina antipolvereMascherina antipolvere
5

How little tin

Caricamento del notebook Jupyter…

Materiali

9

Strumenti richiesti

12

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.

Supporta il Maker acquistando prodotti tramite il suo progetto dove guadagna una Commissione Maker stabilita dai venditori, oppure crea una nuova iterazione di questo progetto e includilo come collegamento nel tuo progetto per condividere i ricavi.

Commenti

(0)

Accedi per partecipare alla discussione

Caricamento commenti...