Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)
Charlie

Creato da

Charlie

1. novembre 2026DE
7
0
0
0
0

Ytterbium: Oxide Reduced by Lanthanum at 1020 °C in Vacuum, Metal Distilled Off (Shindo and Yagi, US 2010/0260640)

Ytterbium boils far more easily than lanthanum. Heated with lanthanum in a vacuum, ytterbium oxide gives up its oxygen to the lanthanum, and the freed ytterbium leaves as vapour and condenses in a cooler zone, while lanthanum oxide stays behind. Result: ytterbium metal ingots; 20 kg of distillate in the patent's run, low in sodium, potassium and lithium. Source: Y. Shindo and K. Yagi, US patent application 2010/0260640 (2010), Example 1. Not given: how much lanthanum, the vacuum, the time, crucible and condenser materials. Picture drawn by Youblob.
Avanzato
1 day

Istruzioni

1

Mix the oxide with lanthanum

Mix ytterbium oxide with lanthanum metal as the reducing agent. Not given: the proportions.

Materiali per questo passaggio:

Ossido di itterbioOssido di itterbio1 as required

Strumenti necessari:

LantanioLantanio
Crogiolo di tantalioCrogiolo di tantalio
2

Reduce in vacuum at 1020 °C

Heat the charge in a vacuum to 1020 °C: Yb2O3 + 2 La -> 2 Yb (vapour) + La2O3. Ours: a vacuum induction furnace; the vacuum level and time are not given.

Strumenti necessari:

Forno a induzioneForno a induzione
Pompa per vuotoPompa per vuoto
Crogiolo di tantalioCrogiolo di tantalio
3

Condense the ytterbium at 200-600 °C

Catch the ytterbium vapour on a condenser held at 200-600 °C. Most of it settles in the 300-500 °C part; the 200-300 °C part carries the least sodium and lithium. Ours: a tantalum condenser plate.

Strumenti necessari:

Piastra condensatrice di tantalioPiastra condensatrice di tantalio
4

Melt into ingots under argon

Take the distillate off the condenser, melt it in a crucible at 950 °C under a slight pressure of argon, and let it solidify into an ingot.

Strumenti necessari:

Crogiolo di tantalioCrogiolo di tantalio
Forno a induzioneForno a induzione
ArgonArgon

Materiali

1

Strumenti richiesti

6

Questo progetto realizza

CC0 Pubblico dominio

Questo progetto è rilasciato sotto CC0. Sei libero di copiare, modificare, distribuire e utilizzare quest'opera per qualsiasi scopo, senza chiedere permesso.