Barium Ferrite Disc Magnet from Natural Magnetite, Presintered at 900 °C (Went, Philips 1956, Ex. 36, Procedure 1)

A barium ferrite magnet made from natural magnetite instead of ferric oxide: barium carbonate and magnetite ground 18 hours, presintered 3 hours at 900 °C, ground again 18 hours, pressed and sintered 2 hours at 1200 °C. Went's rod held 1,450 gauss with a coercive force of 2,425 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 36. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
上級者
2 days

手順

1

Weigh barium carbonate and magnetite

Weigh 9.9 g barium carbonate (0.05 mol) and 46.9 g natural magnetite, Fe3O4 (0.20 mol). Barium carbonate is poisonous if swallowed: gloves and a dust respirator.

このステップの材料:

炭酸バリウム(毒重石)炭酸バリウム(毒重石)9.9 g
磁鉄鉱磁鉄鉱46.9 g

必要な工具:

天秤ばかり天秤ばかり
ゴム手袋ゴム手袋
P100 防じんマスクP100 防じんマスク
2

Grind 18 hours in a ball mill

Grind the mixture in a ball mill for 18 hours. The patent does not say whether wet or dry.

必要な工具:

鉄製ボールミル鉄製ボールミル
P100 防じんマスクP100 防じんマスク
3

Presinter at 900 °C for 3 hours

Fire the ground mixture at 900 °C for three hours and let it cool.

必要な工具:

マッフル炉マッフル炉
蓋付きるつぼ(磁製)蓋付きるつぼ(磁製)
るつぼばさみるつぼばさみ
耐熱手袋耐熱手袋
4

Grind 18 hours in a ball mill

Grind it again in a ball mill for 18 hours. The patent does not say whether wet or dry.

必要な工具:

鉄製ボールミル鉄製ボールミル
P100 防じんマスクP100 防じんマスク
5

Press at 1.5 t/cm²

Press at 1.5 tonnes per cm² (ours: discs instead of a rod).

必要な工具:

油圧プレス油圧プレス
円板プレス金型円板プレス金型
6

Sinter at 1200 °C for 2 hours

Sinter at 1200 °C for 2 hours. The patent gives no atmosphere for this example. Went's rod: 1,450 gauss, 2,425 oersted.

必要な工具:

マッフル炉マッフル炉
るつぼばさみるつぼばさみ
耐熱手袋耐熱手袋
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

必要な工具:

電磁石電磁石
方位磁針方位磁針

材料

2

必要な工具

12

関連ブループリント

これらのブループリントは知識を共有しています — 技術、材料、原理

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...