Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)
Charlie

作成者

Charlie

4. 11月 2026DE
13
0
0
0
0

Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
中級者
30-60 minutes per charge

手順

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

このステップの材料:

自然ビスマス鉱自然ビスマス鉱1 12 cwt per tube charge

必要な工具:

ハンマーハンマー
産業用台秤産業用台秤
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

このステップの材料:

木炭木炭1 powdered, in the pots and for the pot fire

必要な工具:

ビスマス溶離炉ビスマス溶離炉
鋳鉄坩堝鋳鉄坩堝
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

このステップの材料:

薪薪1 about 63 cu ft per 20 cwt of ore

必要な工具:

ビスマス溶離炉ビスマス溶離炉
鉄の丸棒鉄の丸棒
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

必要な工具:

鉄の熊手鉄の熊手
ビスマス溶離炉ビスマス溶離炉
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

必要な工具:

鋳鉄坩堝鋳鉄坩堝
鋳造用の柄杓鋳造用の柄杓
インゴット鋳型インゴット鋳型

材料

3
  • 1 12 cwt per tube charge
    プレースホルダー
  • 1 powdered, in the pots and for the pot fire
    プレースホルダー
  • 1 about 63 cu ft per 20 cwt of ore
    プレースホルダー

必要な工具

8

この設計図で作るもの

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...