Bonded Wire Strain Gauge on Paper: Simmons, 1942

Edward E. Simmons, Jr. of Pasadena patented the bonded wire strain gauge in 1942, US 2,292,549 (filed 1940). A very fine resistance wire is cemented to a member along its entire length, so it stretches and shortens exactly with the surface and its electrical resistance follows the strain. His preferred form: Constantan or Advance wire, about 0.003 inch, wound back and forth on a thin paper, set in Glyptal, then cemented to the member and calibrated.
上級者
Workshop process

手順

1

Wind the filament on thin paper

Use a fine resistance wire such as Constantan or Advance (a copper-nickel alloy, about 45 % nickel and 55 % copper); Simmons used No. 40 gauge, about 0.0031 inch. Wind it back and forth across a thin paper in parallel lengths whose alternate ends are joined, the strands very close together but not touching. A winding jig keeps the filament slightly taut.

このステップの材料:

コンスタンタン線コンスタンタン線1 as required
紙紙1 枚

必要な工具:

巻線治具巻線治具
はさみはさみ
2

Set it in Glyptal

Cover the wound filament with Glyptal and let it dry and harden thoroughly. Filament and paper now form one gauge unit, the filament lying in the plane of the paper surface.

このステップの材料:

グリプタル・アルキド樹脂グリプタル・アルキド樹脂1 as required

必要な工具:

細い筆細い筆
乾燥炉乾燥炉
3

Cement it to the member

Put Glyptal on the surface of the member and wrap the gauge unit on with the strands running in the direction of the strain to be measured, the paper outside. The small amount of Glyptal on the surface insulates the filament from the member. Hold filament and paper in place by wrapping them with thread, then dry and harden the Glyptal thoroughly.

このステップの材料:

グリプタル・アルキド樹脂グリプタル・アルキド樹脂1 as required
木綿糸木綿糸1 as required

必要な工具:

細い筆細い筆
乾燥炉乾燥炉
はさみはさみ
4

Calibrate it

Load the member progressively in a materials testing machine and note the change in the filament's resistance at each load, measured on a Wheatstone bridge in which the filament is one arm. For very fast loads, as in impact tests, an oscillograph takes the place of the galvanometer.

必要な工具:

材料試験機材料試験機
ホイートストンブリッジホイートストンブリッジ
アナログ検流計アナログ検流計
5

Bonding area and signal size

Jupyter ノートブックを読み込み中…

材料

4

必要な工具

7

関連ブループリント

これらのブループリントは知識を共有しています — 技術、材料、原理

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...