Carbon Resistance Ring: Laminated Paper Gelled with 10% Tung Oil, Graphite-Shellac Track
Mallory's quiet volume-control ring (US 2,144,925, 1939). Hard bases were noisy and soft paper ones changed with damp. Their answer: paper rings soaked in 10 % raw tung oil and baked, so the oil gels inside the paper. It shuts out moisture but stays soft and springy, and the wiper runs on it quietly. A graphite paint makes the track, silver paint the ends.
The picture: the patent's drawing (Fig. 3).
中級者
1 day
手順
1
1
Punch rings from three-ply paper
Punch rings from three-ply paper
The base is three papers stuck into one sheet: litho paper at the back, newsprint in the middle, manila on the face that takes the track. Punch rings from it. Ours: a punch press with a ring die.
このステップの材料:
三層積層紙1 個必要な工具:
パンチプレス
リング打ち抜きダイ
ゴム手袋2
2
Soak 1 hour in 10 % tung oil in naphtha
Soak 1 hour in 10 % tung oil in naphtha
Soak the rings for about one hour in about 10 % raw tung oil in naphtha. Use raw oil, not heat-bodied or treated oil, so it can still gel.
このステップの材料:
桐油10 parts必要な工具:
ナフサ
ガラスビーカー
天秤ばかり
撹拌具
全面形呼吸用保護具
ゴム手袋3
3
Air-dry, then bake at 210–250 °C
Air-dry, then bake at 210–250 °C
Dry the rings in air for two hours or more, then bake 15 to 30 minutes at 210 to 250 °C. The oil gels in the paper's pores; the paper stays pliable.
必要な工具:
乾燥炉
オーブン用温度計
耐熱手袋4
4
Spray the graphite track
Spray the graphite track
Spray on the resistance paint, for example graphite in a shellac binder. The patent gives no proportions. The track can be tapered in thickness, width or mix to shape the resistance curve.
このステップの材料:
黒鉛粉末1 as required
シェラック1 as required必要な工具:
スプレーガン
空気圧縮機
全面形呼吸用保護具
ゴム手袋5
5
Paint silver ends, bake at 220 °C
Paint silver ends, bake at 220 °C
Spray or paint the two end terminals with silver particles in shellac. Dry, then bake at about 220 °C to cure and harden the track. The slight warp from soaking flattens out again.
このステップの材料:
銀導電塗料1 as required必要な工具:
スプレーガン
乾燥炉
オーブン用温度計
耐熱手袋材料
5- 1 個プレースホルダー
- 10 partsプレースホルダー
- 1 as requiredプレースホルダー
- 1 as requiredプレースホルダー
- 1 as requiredプレースホルダー
この設計図で作るもの
関連ブループリント
これらのブループリントは知識を共有しています — 技術、材料、原理
CC0 パブリックドメイン
このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。
メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。