Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)

Barium titanate with 3 mole % nickel stannate is calcined, pressed into small discs and fired hard. Silver is fired onto both faces and a lead soldered to each, giving ceramic disc capacitors of high capacity for their size. Result: discs 3/8 inch across and about 1/10 inch thick with a dielectric constant averaging 2380 and a dissipation factor of 0.58 %. Between 25 and 85 °C the dielectric constant rose at most 17 % and fell at most 7 %. Source: W. W. Coffeen (Metal & Thermit Corp.), US 2,789,061 (1957). Unknown: how the barium titanate, the nickel stannate and the tinned lead wire are made; the patent uses them ready-made. Picture: Wikimedia Commons.
上級者
10 days

手順

1

Weigh and slurry

Weigh 19.32 g of barium titanate and 0.68 g of hydrated nickel stannate (about NiSnO3·2H2O), which is 97 mole % BaTiO3 and 3 mole % NiSnO3. Slurry them with 50 cc of distilled water. The patent prefers 2 to 4 mole % nickel stannate; 1 to 15 % works.

このステップの材料:

チタン酸バリウムチタン酸バリウム19.32 g
スズ酸ニッケルスズ酸ニッケル0.68 g

必要な工具:

蒸留水蒸留水
精密デジタルスケール精密デジタルスケール
蒸発皿蒸発皿
2

Dry, sieve and calcine

Dry the slurry, crush it to pass a 50 mesh screen, moisten it with 5 % of a 2 1/2 % starch solution and press it into one slug. Calcine the slug for one hour at 1600 °F (871 °C). Ours: potato starch, a drying oven, mortar and pestle.

必要な工具:

馬鈴薯でんぷん馬鈴薯でんぷん
乾燥炉乾燥炉
乳鉢と乳棒乳鉢と乳棒
ふるい(粗目)ふるい(粗目)
油圧プレス油圧プレス
高温窯高温窯
3

Press the discs

Grind the calcine to pass a 325 mesh screen, moisten it again with starch solution, and press small discs 3/8 inch in diameter and about 1/10 inch thick at 20,000 pounds per square inch.

必要な工具:

乳鉢と乳棒乳鉢と乳棒
目の細かいふるい目の細かいふるい
馬鈴薯でんぷん馬鈴薯でんぷん
油圧プレス油圧プレス
円板プレス金型円板プレス金型
4

Fire on platinum

Fire the discs on platinum foil at 2400 °F (1316 °C) for one hour. They come out with zero absorption.

必要な工具:

高温窯高温窯
白金白金
5

Silver and lead

Paint silver paint on both faces and fire the discs at 1350 °F (732 °C) for one hour. Solder tinned copper lead wires directly to the silver electrodes. Age at least a week before measuring. Ours: a fine brush and a soldering iron.

このステップの材料:

焼付け銀ペイント焼付け銀ペイント1 both faces
すずめっき銅線すずめっき銅線2 leads per disc
はんだ線はんだ線1 a little

必要な工具:

先の細い筆先の細い筆
高温窯高温窯
はんだごてはんだごて

材料

5

必要な工具

14

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...