Die Casting
手順
Cast into sand for comparison
Cast into sand for comparison
Make the baseline before improving on it. Work with a low-melting alloy only.
- Press a pattern into damp casting sand to make a cavity.
- Melt pewter and pour it in.
- Break out the casting and examine the surface and edges.
このステップの材料:
Pewter Ingot500 g
Instant-Read Thermometer1 個Make a reusable two-part die
Make a reusable two-part die
A permanent mould that opens, in metal or high-temperature board.
- Cut matching halves with the cavity split across a chosen parting line.
- Add locating pins so the halves register exactly.
- Cut a sprue to admit metal and thin vents at the far extremities.
このステップの材料:
Firebricks2 個Add draft, and learn why
Add draft, and learn why
No cavity wall may be parallel to the opening direction.
- Taper every wall by a degree or two so it narrows away from the parting line.
- Cast once with a deliberately parallel wall and try to open the die.
- Compare with the tapered version.
Add pressure and compare the detail
Add pressure and compare the detail
Pressure is what separates die casting from gravity permanent-mould casting.
- Fill once by gravity alone and examine fine detail and corners.
- Fill again while applying steady pressure at the sprue as it solidifies.
- Compare edge sharpness and any porosity when you cut a casting through.
このステップの材料:
Zinc Ingot 99.9% Pure 1 lb1 ingotHistory and context
History and context
Sturges patented a hand-operated die casting machine in 1849, and the application was printing type. Type demands exactly what die casting provides — identical pieces, crisp fine detail, and enormous quantities — and the Linotype and Monotype machines later cast type on demand as an integral part of typesetting.
Zinc made it general. Zinc alloys melt low enough to be handled by a hot-chamber machine, where the injection mechanism sits in the molten metal itself, giving very fast cycles. Aluminium attacks steel injection parts at temperature, so it uses cold-chamber machines where metal is ladled in for each shot — slower, and the reason aluminium castings cost more than zinc ones.
The honest weakness is porosity. Injecting metal at high speed entrains air, which is trapped as fine bubbles through the casting. That makes conventional die castings hard to weld or heat-treat, because trapped gas expands and blisters. Vacuum die casting and squeeze casting exist specifically to address it — and it is why a structural part is often forged rather than die cast.
Safety, plainly: molten metal and moisture are a serious combination — water trapped in a mould flashes to steam and throws metal violently. Everything that touches melt must be bone dry and preheated. Do not attempt this with zinc or aluminium without proper equipment; the pewter steps here are at a temperature a workshop can handle safely with full face and hand protection.
材料
4- 500 gプレースホルダー
- プレースホルダー
- 2 個プレースホルダー
- 1 ingotプレースホルダー
CC0 パブリックドメイン
このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。
メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。