Goatskin Leather Tanned with Sumac, the Morocco Way
Morocco leather is goatskin tanned with sumac: light, supple and fine-grained. Andrew Ure (1839) gives the method: bran and lime to loosen the hair, the skin scraped clean, then sewn into a bag, grain outside, and floated in sumac liquor for a day. Oiled and curried, it takes the pebbled grain used for gloves and book covers.
The picture: early 18th-century calf bindings inlaid with panels of coloured morocco.
上級者
Two to three weeks
手順
1
1
Soak in bran water
Soak in bran water
Steep the skins a few days in water with bran stirred in, until it ferments. Work them on the beam, soak 12 hours in fresh water and rinse.
このステップの材料:
山羊の原皮6 個
小麦ふすま2 kg
水100 リットル必要な工具:
木製のたらい
肉削ぎ台2
2
Lime and dehair
Lime and dehair
Steep them in weak lime water until the hair pulls out easily. Scrape the hair off on the beam with the back of the fleshing knife and wash them in running water.
このステップの材料:
消石灰2 kg
水60 リットル必要な工具:
木製のたらい
肉削ぎ台
肉削ぎ包丁
ゴム手袋3
3
Flesh and clean out the lime
Flesh and clean out the lime
Shave off flesh and fat with the fleshing knife and trim the edges. Rub the grain hard with a flat stone to press out lime, then a night and a day in a fresh bran bath.
このステップの材料:
小麦ふすま1 kg
水50 リットル必要な工具:
肉削ぎ包丁
肉削ぎ台
砥石 1000 番
木製のたらい4
4
Sew into bags
Sew into bags
Sew each skin edgewise into a bag with the grain outside, leaving a small opening.
このステップの材料:
亜麻糸20 m必要な工具:
縫い針5
5
Tan in sumac
Tan in sumac
Fill each bag with strong sumac liquor and close it; float the bags in a tub of the same liquor and keep them moving by hand for four hours. Drain, refill and tan again: about 24 hours in all.
このステップの材料:
スマックの葉(乾燥)5.4 kg
水60 リットル必要な工具:
木製のたらい
天秤ばかり6
6
Open, rinse and dry
Open, rinse and dry
Unstitch the skins, rinse them, beat them soft, drain them and hang them to dry. While still damp, sponge a thin film of linseed oil on the grain so they stay glossy and do not go horny.
このステップの材料:
亜麻仁油0.2 リットル必要な工具:
スポンジ7
7
Curry and grain
Curry and grain
Thin the flesh side where needed and smooth the damp skin. Then work it on the flesh side with a cork-faced board, in several directions, to raise the pebbled grain (Ure: the curriers' pommel faced with cork).
必要な工具:
肉削ぎ包丁
コルクシート8
8
Sumach for the batch
Sumach for the batch
Jupyter ノートブックを読み込み中…
9
9
Limits
Limits
The process and the sumac rate are Ure's; we leave out his dyeing (cochineal, iron, indigo) and give the undyed leather. Bath volumes are ours.
材料
7- 6 個プレースホルダー
- 2 kgプレースホルダー
- 270 リットルプレースホルダー
- 2 kgプレースホルダー
- 20 mプレースホルダー
- 5.4 kgプレースホルダー
- 0.2 リットルプレースホルダー
この設計図で作るもの
関連ブループリント
これらのブループリントは知識を共有しています — 技術、材料、原理
CC0 パブリックドメイン
このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。
メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。