Lead-Free Plumbing Solder: Tin with 0.7 % Copper, Cast in Bars
Lead has been banned from drinking-water plumbing solder in the US since 1974; tin with a little copper took its place. Tin with 0.7 % copper melts at 227 °C, higher than the old tin-lead. Melt the tin, dissolve the copper in it and cast it into bars, the thick form plumbers use.
The picture: soldering a copper pipe joint with a torch.
中級者
Two hours
手順
1
1
Weigh
Weigh
Weigh 99.3 parts tin to 0.7 parts copper (step 5). Cut the copper wire into short pieces.
このステップの材料:
錫のインゴット993 g
銅線7 g必要な工具:
天秤ばかり
金切りばさみ2
2
Melt and alloy
Melt and alloy
Melt the tin in an iron crucible on the forge hearth under a thin layer of charcoal dust (ours). Drop in the copper pieces and stir with an iron rod, keeping it hot, until no copper is left undissolved.
必要な工具:
鋳鉄坩堝
炉床(鍛冶の火)
木炭
鉄の丸棒
るつぼばさみ
溶接用手袋
保護めがね3
3
Cast bars
Cast bars
Skim off the charcoal and pour the alloy into a warmed ingot mould. Knock the bars out when cold.
必要な工具:
インゴット鋳型
るつぼばさみ
溶接用手袋
保護めがね4
4
Label
Label
Scratch a mark on each bar so it is never mixed with lead solder.
必要な工具:
鉄の丸棒5
5
Tin and copper
Tin and copper
Jupyter ノートブックを読み込み中…
この設計図で作るもの
関連ブループリント
これらのブループリントは知識を共有しています — 技術、材料、原理
CC0 パブリックドメイン
このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。
メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。