Forged Square-Neck Door Bolt and Nut, Threaded with a Screw-Plate (Moxon, 1677)
Joseph Moxon's 1677 way to make the screw bolt for a door: a square iron bar forged down to a square neck and round pin, the head cut off with a chisel, the pin threaded with a screw-plate, and a punched iron nut threaded with a tap. The square neck sits in a square hole so the bolt cannot turn while the nut is tightened.
中級者
About an hour per bolt
手順
1
1
Choosing the hole
Choosing the hole
Jupyter ノートブックを読み込み中…
2
2
Read Mechanick Exercises
Read Mechanick Exercises
"The Shank of the Screw for Doors and many other purposes must be Forged square near the Head, because it must be let into a square hole that it may not twist about when the Nut is turned about hard upon the Screw-Pin."
3
3
Forge the square neck
Forge the square neck
Take a square iron bar as near the size of the head as you can. At a flame (white) heat lay the shank length flat on the near side of the anvil and hammer it down to thickness; do not strike over the edge or you cut the iron. Reheat, turn it, and hammer the other two sides close up to the head.
このステップの材料:
錬鉄の棒1 個必要な工具:
鍛冶炉
金床
ハンマー
鍛冶やっとこ4
4
Round the pin, cut the head
Round the pin, cut the head
Hammer down the corners of the part meant for the thread and round it. Set the chisel at the head thickness, strike half through, turn and cut each side half through until it comes off. Square the shoulder: reheat, grip in square-nosed tongs, set the shank in the vice with the shoulder on the jaws, and hammer the head.
必要な工具:
鍛冶炉
金床用たがね
鍛冶やっとこ
重量級万力
ハンマー5
5
Punch the nut
Punch the nut
Forge a nut blank from the bar. Harden the point of a steel punch of the hole's size (no tempering: the hot iron softens it). At a blood-red heat punch from one side until the far side bulges, turn it, set it flat, and punch through over the hole of a bolster. Dip the punch in water whenever it changes colour. Let forged work cool on the floor or hearth; never quench it.
このステップの材料:
錬鉄の棒1 個必要な工具:
鍛冶炉
金床
熱間ポンチ
ハンマー
焼き入れ桶
鍛冶やっとこ6
6
Thread the pin
Thread the pin
File the shank and head, file the pin round, and taper its end by the depth of the screw-plate's threads. Find the screw-plate hole the pin just slides through, turn the pin in it, and file off the marks it cuts: the pin is then true. Set the bolt head down in the vice, press the next smaller hole (groove diameter equal to the pin) hard down on it, and turn the plate evenly.
必要な工具:
やすり(手やすり)
重量級万力
ねじ切りタップダイスセット7
7
Tap the nut
Tap the nut
Fit the tap to the round hole of the nut; it must match the pin (try it in the same screw-plate hole). Set the nut flat in the vice and turn the tap hard round by its handle, or by the square hole near the screw-plate handle, until it cuts the thread.
必要な工具:
重量級万力
ねじ切りタップダイスセット8
8
Troubleshooting
Troubleshooting
Screw bolt troubleshooting.
Flow
Loading...
9
9
History and honest limits
History and honest limits
From Joseph Moxon, **Mechanick Exercises, or the Doctrine of Handy-Works** (1677), Smithing, Numb. I pp. 10-11 and Numb. II pp. 29-31 (checked on the archive.org scan mechanickexercis00moxo). He gives no sizes or nut shape; the metric example and the tool heads are ours.
この設計図で作るもの
関連ブループリント
これらのブループリントは知識を共有しています — 技術、材料、原理
CC0 パブリックドメイン
このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。
メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。