Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)

The file for sharpening saw teeth as Sheffield made it by hand: a three-square (triangular) bar of cast steel, not tapering, forged in a V-shaped boss, its teeth cut one by one with a chisel and hammer, then hardened under a coat of animal carbon and salt and quenched in cold spring water. Ure says saw files in particular should be hardened with the carbon mixture, so they will cut iron and steel. Not given: sizes and teeth per inch. Source: A. Ure, Dictionary of Arts, Manufactures, and Mines (1839), File. Picture: our drawing.
上級者
Unknown

手順

1

Forge the blank

Draw cast steel out square at the forge, then lay it with one angle down in a boss whose recess has two sides meeting at an angle, so the hammer forms one side and the boss the other two. Keep it the same size along its length (saw files are not tapered).

このステップの材料:

るつぼ鋼るつぼ鋼1 cast steel bar
不明な寸法不明な寸法1 個

必要な工具:

鍛冶炉鍛冶炉
鍛冶ばさみ(やっとこ)鍛冶ばさみ(やっとこ)
下型スエージ下型スエージ
ハンマーハンマー
大ハンマー大ハンマー
2

Cut the teeth

On an anvil with a flat, even face, hold the file down with a leather strap over each end, the workman's feet in the straps like stirrups. Cut the teeth with a chisel a little broader than the file, sharpened to about 20 degrees, struck with a hammer of 1 to 6 lb. For single cut, run a fine file lightly over the teeth to take off the roughness; for double cut, cut a second set nearly at right angles to the first.

必要な工具:

鋼の金床鋼の金床
革ひも革ひも
たがねたがね
ハンマーハンマー
金工ヤスリ金工ヤスリ
3

Cut the other sides

To cut the next side, lay the file in a piece of lead-tin alloy with an angular groove, so the teeth already cut are not spoiled on the anvil.

必要な工具:

錫鉛はんだ錫鉛はんだ
鋼の金床鋼の金床
たがねたがね
ハンマーハンマー
4

Coat for hardening

Distil shoemakers' and curriers' leather refuse in an iron still and powder the bright coal left. Grind about equal parts by bulk of this carbon and salt to the consistence of cream with water and cover the file with it.

必要な工具:

鉄のレトルト鉄のレトルト
塩塩
水水
5

Harden

Hold the file by the tang in a fire of very small cokes, drawing it out often, until it is an even cherry red from tang to point. Plunge it straight down, quickly, into clear spring water as cold as possible.

必要な工具:

鍛冶炉鍛冶炉
冶金用コークス冶金用コークス
鍛冶ばさみ(やっとこ)鍛冶ばさみ(やっとこ)
水水
6

Clean and oil

Brush the file with water and powdered cokes until clean and metallic, wash it in two or three waters to take off all the salt, dip it in lime-water, dry it quickly before the fire and oil it while warm with olive oil containing a little oil of turpentine.

必要な工具:

冶金用コークス冶金用コークス
水水
石灰水石灰水
オリーブオイルオリーブオイル
テレビン油テレビン油

材料

2
  • 1 cast steel bar
    プレースホルダー
  • プレースホルダー

必要な工具

17

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...