Eston H. Smith of Indianapolis received US 2,543,206, dated 27 February 1951, for a flat wood-boring bit made for the high speeds of an electric drill, 2,000 to 3,500 revolutions a minute. A flat plate on a thin stem has edges square to its faces and exactly the same width all the way down. A long flat pilot below it keeps the bit centred until it is through. With no screw feed it can bore at an angle, into another hole, or overlapping one, without splitting the wood. The thin stem leaves room for the shavings to come out. We forge his 3/4 inch bit to his figures, with 1/2 and 1 inch bits beside it.
中級者
About 1 day

手順

1

His figures in millimetres

Jupyter ノートブックを読み込み中…
2

Read US 2,543,206

"It is extremely important however that these edges 15 and 16 be of exactly constant width from top to bottom, else the holes will not be bored true, and chattering and heating might develop."
3

Forge the blades

Cut three 170 mm lengths of 10 mm octagonal tool steel. Heat 50 mm of one end to a bright orange in the forge and flatten it on the anvil to about 3 mm thick, centred on the bar. Hammer across it with the peen to spread it wider than the bit, about 2 mm over its size: 15, 21 and 27 mm. Draw the neck down smoothly where the blade meets the bar and keep the blade in line with it. Reheat as soon as the colour fades to red. Finally heat each one to a cherry red and let it cool slowly in the air, to soften it for filing.

このステップの材料:

工具鋼八角棒工具鋼八角棒3 個

必要な工具:

金切りのこ(ハクソー)金切りのこ(ハクソー)
万力(ベンチバイス)万力(ベンチバイス)
鍛冶炉鍛冶炉
金床金床
鍛造槌鍛造槌
鍛冶ばさみ(やっとこ)鍛冶ばさみ(やっとこ)
溶接用手袋溶接用手袋
保護めがね保護めがね
4

Print the grinding template

Full-size A4 template: the outlines of the 1/2, 3/4 and 1 inch bits with the long flat pilot. Print at 100 %; its 50 mm bar must measure 50 mm.
デザインファイルPDFCC0 - Free
5

Grind the outline

Glue each outline on its blade, centred on the bar, and grind to the lines on the bench grinder, dipping the steel in water often. Grind the faces flat and parallel to 2.4 mm (3/32 inch). Grind the plate's two side edges and the pilot's two side edges square to the faces and exactly parallel; check the plate's width with the caliper at the top and the bottom, it must not change. Grind three flats on the end of the stem, 20 mm long, for the chuck's jaws.

必要な工具:

インクジェットプリンターインクジェットプリンター
接着剤接着剤
卓上グラインダー卓上グラインダー
焼き入れ桶焼き入れ桶
水水
ヤスリセットヤスリセット
万力(ベンチバイス)万力(ベンチバイス)
デジタルノギス 6インチデジタルノギス 6インチ
保護めがね保護めがね
6

Grind the clearances

The bit turns clockwise seen from the stem. Grind each cutting edge either side of the pilot square to the axis, with no top rake, and a clearance of 15 degrees behind it, on the face that trails. Grind the pilot's two point edges to 58 degrees included and give each a clearance of 9 degrees the same way. Leave a 1 mm flat at the tip, square to the axis.

必要な工具:

卓上グラインダー卓上グラインダー
焼き入れ桶焼き入れ桶
水水
ヤスリセットヤスリセット
万力(ベンチバイス)万力(ベンチバイス)
7

Harden and temper

Heat the blade and the neck evenly to a cherry red, until a magnet no longer sticks to it, and quench it straight down in water, moving it up and down. Rub the faces bright with a stone. Heat the shank gently 30 mm behind the blade and watch the colours run down; quench again as soon as a dark straw colour reaches the shoulders and the point. Do the other two.

必要な工具:

鍛冶炉鍛冶炉
鍛冶ばさみ(やっとこ)鍛冶ばさみ(やっとこ)
小さな磁石小さな磁石
焼き入れ桶焼き入れ桶
水水
砥石砥石
溶接用手袋溶接用手袋
保護めがね保護めがね
8

Sharpen and test

Hone the cutting edges on the shoulders and the point with the stone, keeping their angles, and take the burr off. Chuck a bit by its flats and bore a scrap of hardwood: it should start on the point without wandering, cut two clean shavings from the shoulders and leave a round hole of its own size; check it with the caliper.

必要な工具:

砥石砥石
コードレスドリルコードレスドリル
堅木の板堅木の板
デジタルノギス 6インチデジタルノギス 6インチ
保護めがね保護めがね
9

Troubleshooting

Long-pilot bit troubleshooting.

Flow

Loading...
10

History and honest limits

**Eston H. Smith** of Indianapolis, assignor to Benjamin B. Aufderheide, US 2,543,206, dated 27 February 1951, filed 23 July 1948. He claimed a flat plate on a stem with a flat pilot, their edge faces at ninety degrees to their faces, a pilot point of 55 to 60 degrees with 8 to 10 degree clearances, and cutting edges square to the pilot with a clearance of between 15 and 20 degrees (his text says 10 to 20). His figures are for the 3/4 inch bit; the 1/2 and 1 inch bits are ours, with his pilot and edge height. His stem is about 1/4 inch with flats; ours is octagonal tool steel with three ground flats. He gives no material or heat treatment; those are ours.

材料

1

必要な工具

19

設計ファイル

1

関連ブループリント

これらのブループリントは知識を共有しています — 技術、材料、原理

CC0 パブリックドメイン

このブループリントはCC0で公開されています。許可を求めずに、自由にコピー、修正、配布、あらゆる目的で使用できます。

メイカーを応援するには、ブループリント経由で製品を購入してください。メイカーには メイカーコミッション がベンダーにより設定されています。または、このブループリントの新しいイテレーションを作成し、自分のブループリントにコネクションとして含めて収益を共有できます。

ディスカッション

(0)

ログイン してディスカッションに参加

コメントを読み込み中...